Cerium-zirconium solid solution catalyst for decomposing CO2 and preparation method thereof

The Ce/Zr ratio optimization of the cerium-zirconium solid solution catalyst prepared by the evaporation-induced self-assembly method has solved the problem of volatility and inactivation of the catalyst in the existing CO2 conversion catalytic system, and achieved an efficient and stable CO2 decomposition reaction, especially Ce0. The cyclic stability and catalytic activity of 75Zr0.25O2 material has excellent performance.

CN118949969APending Publication Date: 2024-11-15BOZHOU SHANGDA ENG TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410879936.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing CO2 conversion catalytic system has problems such as easy volatility of the catalyst, high thermal reduction temperature, and inactivation of sintering, which makes the reaction difficult to continue, and the stability and reaction performance of the CeO2/Ce2O3 system need to be further improved.

Method used

The evaporation-induced self-assembly method is used to prepare cerium-zirconium solid solution catalysts with different Ce/Zr ratios, optimize the Ce/Zr ratio to improve catalytic activity and cycle stability, and the structure and reduction performance of the catalyst are affected by adjusting the Ce/Zr ratio, and the high-quality is prepared. Catalytic activity and stability of CexZr1-xO2 catalyst.

Benefits of technology

The catalytic activity and cycle stability of CO2 two-step thermochemical method are improved, ensuring the efficiency and long-term stability of the catalyst in high-temperature decomposition reactions. The cyclic stability of Ce0.75Zr0.25O2 material has the best catalytic activity, and the catalytic activity is Ce Optimal when /Zr=1:1.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949969A_ABST
    Figure CN118949969A_ABST
Patent Text Reader

Abstract

The invention provides a cerium-zirconium solid solution catalyst for decomposing CO2 and a preparation method of the cerium-zirconium solid solution catalyst, and aims to improve the activity and stability of the catalyst in a CO2 conversion process by optimizing the composition and the structure of the catalyst and provide a new way for realizing efficient resource utilization of CO2. The invention explores the structure (x is 0 or 1) of the Ce / Zr ratio to CexZr1-xO2, and finds that along with the increase of the Ce / Zr ratio, the crystal structure of the cerium-zirconium solid solution catalyst is converted from a tetragonal phase to a cubic phase, the grain size is reduced along with the increase of the Zr content, and the specific surface area is increased along with the increase of the Zr content. And along with the increase of the Ce / Zr ratio, the number of oxygen holes and the reduction performance of the cerium-zirconium solid solution catalyst are firstly increased and then reduced. Besides, in a two-step thermochemical method CO2 decomposition reaction experiment, the catalytic activity of the cerium-zirconium solid solution catalyst is firstly increased and then reduced along with the increase of the proportion of Ce / Zr, the catalytic activity is the best when the proportion of Ce / Zr is 1: 1, and the cerium-zirconium solid solution catalysts in all proportions keep good thermal stability and do not have serious inactivation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of CO2 emission reduction and resource utilization, and in particular to a cerium-zirconium solid solution catalyst for decomposing carbon dioxide (CO2) and a preparation method thereof. Background Art

[0002] With the continuous rapid economic growth, the demand for energy is increasing day by day, and the energy shortage problem has become the focus of global attention. At the same time, the greenhouse gas emissions such as carbon dioxide (CO2) generated by the large-scale consumption of fossil energy have had a profound impact on global warming. Therefore, it is particularly urgent to find new energy alternatives and effective ways to reduce CO2 emissions.

[0003] As a widely available and cheap resource, CO2 resource utilization has become one of the effective ways to solve the energy crisis and climate warming. By using technical means to convert CO2 into high value-added products such as carbon monoxide, methanol, carbonates, olefins, gasoline and diesel, it can not only reduce CO2 emissions, but also partially alleviate the dependence on traditional fossil energy such as coal, oil and natural gas.

[0004] As a clean and renewable energy source, solar energy provides an ideal energy source for the resource utilization of CO2. At present, the technologies for CO2 conversion using solar energy mainly include photoelectrocatalysis, photocatalysis, artificial simulation of photosynthesis and photothermal conversion. Among them, photothermal conversion technology has attracted widespread attention because it can utilize the entire solar energy spectrum and has high energy conversion efficiency.

[0005] However, there are still some problems with the CO2 conversion catalytic systems reported so far. For example, Zn-based catalysts are volatile during the reaction, and Zn vapor is easily combined with O2 and reoxidized, making it difficult for the reaction to continue. SnO-based catalysts also face problems such as low melting point and easy combination with O2. The Fe3O4 / FeO system has problems such as high thermal reduction temperature and easy sintering and deactivation of the material. Although CeO2 has a fast reaction rate, it also faces the risk of high thermal reduction temperature and sintering deactivation.

[0006] In order to solve the above problems, researchers are constantly exploring new catalytic systems and preparation methods. The CeO2 / Ce2O3 system shows good application potential because it does not vaporize or sublimate during the reaction and has a fast reaction rate. However, its stability and reaction performance need to be further improved. Summary of the invention

[0007] Based on the above background, the present invention provides a cerium-zirconium solid solution catalyst for decomposing CO2 and a preparation method thereof. The present invention finds the effect of Ce / Zr ratio on Ce x Zr 1-xTaking into account the influence of O2's structure (x is 0 or 1), reduction properties and activity in high-temperature decomposition of CO2, a series of cerium-zirconium solid solutions with different Ce / Zr ratios were prepared by evaporation-induced self-assembly method to improve their catalytic activity and cyclic stability in the two-step thermochemical method of CO2.

[0008] The first aspect of the present invention is to provide a method for preparing a cerium-zirconium solid solution catalyst for decomposing CO2, the steps comprising:

[0009] Provide a P123 template;

[0010] The template of P123, cerium salt (Ce 3+ ), zirconium salt (Zr 4+ ) are mixed in a reaction solvent to obtain an intermediate product; the intermediate product is heat-treated to obtain a cerium-zirconium solid solution catalyst.

[0011] In a preferred embodiment, the method for preparing the P123 template comprises the following steps:

[0012] P123 was stirred in anhydrous ethanol.

[0013] Preferably, the stirring time is 1-8 h, more preferably 2-6 h, more preferably 4-5 h.

[0014] In a preferred embodiment, the ratio of cerium salt, zirconium salt and P123 is: 80-160g P123 per 1mol of cerium salt and zirconium salt, preferably 90-130g P123, and more preferably 100-120g P123.

[0015] In a preferred embodiment, the cerium salt may be one or more combinations selected from Ce(NO3)3, Ce2(CO3)3, Ce2(SO4)3, CeCl3, and CeBr3.

[0016] More preferably, the cerium salt is a water-soluble or alcohol-soluble salt.

[0017] More preferably, the cerium salt is provided in the form of its hydrate, aqueous solution or alcohol solution.

[0018] In a preferred embodiment, the zirconium salt may be one or more combinations selected from Zr(NO3)4, Zr(SO4)2, Zr(CO3)2, ZrCl4, and ZrBr4.

[0019] More preferably, the zirconium salt is a water-soluble or alcohol-soluble salt.

[0020] More preferably, the zirconium salt is provided in the form of its hydrate, aqueous solution or alcohol solution.

[0021] More preferably, the Ce / Zr ratio is 1:(0.1-5), more preferably 1:(0.15-4.5), more preferably 1:(0.2-4), such as 1:4, 1:3, 1:2, 2:1, 3:1, 4:1.

[0022] In a preferred embodiment, the P123, cerium salt (Ce 3+ ), zirconium salt (Zr 4+ ) reaction solvents include one or more combinations of N,N-dimethylformamide solution, methanol, ethanol, ether, tetrahydrofuran, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, and ionic liquids (such as 1-butyl-3-methylimidazolium hexafluorophosphate).

[0023] In a preferred embodiment, the P123, cerium salt (Ce 3+ ), zirconium salt (Zr 4+ ) is mixed at a temperature of 20-100°C, more preferably 30-80°C, more preferably 40-60°C.

[0024] In a preferred embodiment, the P123, cerium salt (Ce 3+ ), zirconium salt (Zr 4+ ) has a mixing time of 2-55 h, more preferably 4-50 h, more preferably 6-48 h.

[0025] In a preferred embodiment, the P123, cerium salt (Ce 3+ ), zirconium salt (Zr 4+ ) The reaction solvent was also evaporated during the mixing process.

[0026] In a preferred embodiment, the intermediate product is a xerogel.

[0027] In a preferred embodiment, the heat treatment comprises calcining or roasting.

[0028] Preferably, the heat treatment is calcination, and the calcination temperature is 500-1000°C, more preferably 550-800°C, and more preferably 600-700°C.

[0029] More preferably, the calcination time is 1-8 h, more preferably 2-6 h, more preferably 4-5 h.

[0030] More preferably, the heating rate of the calcination is 0.1-2°C / min, more preferably 0.2-1.5°C / min, more preferably 0.5-1°C / min.

[0031] The present invention also provides a cerium-zirconium solid solution catalyst for decomposing CO2, the molecular formula of which is: Ce r Zrs O t , wherein r:s:t is (0.1-1):(0.1-1):2, preferably (0.2-1):(0.2-1):2, more preferably (0.2-0.8):(0.2-0.8):2, for example, r:s:t can be one or more of 0.2:0.8:2, 0.33:0.67:2, 0.67:0.33:2, 0.75:0.25:2, 0.8:0.2:2.

[0032] Preferably, the cerium-zirconium solid solution catalyst for decomposing CO2 is obtained based on the preparation method described in the present invention.

[0033] In the present application, P123 is a triblock copolymer, which is a nonionic amphiphilic triblock copolymer of the polyoxyethylene-polyoxypropylene-polyoxyethylene (PEO-PPO-PEO) type. Preferably, the P123 can form micelles or liquid crystal phases at a set temperature and concentration.

[0034] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0035] The present invention provides a cerium-zirconium solid solution catalyst for decomposing CO2 and a preparation method thereof, aiming to improve its activity and stability in the CO2 conversion process by optimizing the composition and structure of the catalyst, thereby providing a new way to achieve efficient resource utilization of CO2. The applicant found that the Ce / Zr ratio has an important effect on the x Zr 1-x O2 structure (x is 0 or 1), and found that as the Ce / Zr ratio increases, the crystal structure of the cerium-zirconium solid solution catalyst changes from tetragonal phase to cubic phase, the grain size decreases with the increase of Zr content, and the specific surface area increases with the increase of Zr content. And as the Ce / Zr ratio increases, the number of oxygen vacancies and reduction performance of the cerium-zirconium solid solution catalyst first increases and then decreases. In addition, in the two-step thermochemical CO2 decomposition reaction experiment, the catalytic activity of the cerium-zirconium solid solution catalyst first increases and then decreases with the increase of Ce / Zr ratio. The catalytic activity is best when Ce / Zr=1:1. The cerium-zirconium solid solution catalysts at all ratios maintain good thermal stability and do not show serious deactivation. Among them, Ce 0.75 Zr 0.25 O2 material has the best cyclic stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The X-ray diffraction (XRD) spectra of samples with different Ce / Zr ratios obtained by implementing the present invention.

[0037] Figure 2 Raman spectrum of the cerium-zirconium solid solution obtained by the present invention (a) Ce0.2 Zr 0.8 O2,(b)Ce 0.33 Zr 0.67 O2,(c)Ce 0.67 Zr 0.33 O2,(d)Ce 0.75 Zr 0.25 O2, (e)Ce 0.8 Zr 0.2 O2.

[0038] Figure 3 XPS spectra of (a) Ce 3d, (b) Zr 3d, and (c) O 1s of the cerium-zirconium solid solution obtained by implementing the present invention.

[0039] Figure 4 This is the H2-TPR spectrum of the cerium-zirconium solid solution obtained by implementing the present invention.

[0040] Figure 5 The TGA curves of CO2 decomposition cyclic reaction of cerium-zirconium solid solution with different Ce / Zr ratios before cyclic reaction obtained by implementing the present invention.

[0041] Figure 6 The average CO production and average reduction degree of the cerium-zirconium solid solution material obtained by the implementation of the present invention.

[0042] Figure 7 The average reduction degree of the cerium-zirconium solid solution material obtained by the present invention is 3+ / Ce 4+ Molar ratio relationship diagram. DETAILED DESCRIPTION

[0043] The embodiments of the present invention provide a cerium-zirconium solid solution catalyst for decomposing CO2 and a preparation method thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0044] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0045] Example

[0046] (1) Using the evaporation-induced self-assembly method: a certain proportion of P123 was dissolved in anhydrous ethanol and stirred continuously for 4 hours (1 g of P123 was used as a template for every 0.01 mol of nitrate). Afterwards, a certain proportion of Ce(NO3)3·6H2O and Zr(NO3)4·5H2O was added to the above solution in sequence and stirred for 5 hours. Then, the solution was transferred to a constant temperature and humidity drying oven and the solvent was evaporated at 60°C and a relative humidity of 20% for 48 hours. The dry gel was heated at a rate of 1°C min -1 The cerium-zirconium solid solution materials with Ce / Zr ratios of 1:4, 1:2, 2:1, 3:1 and 4:1 were prepared and are denoted as Ce 0.2 Zr 0.8 O2、Ce 0.33 Zr 0.67 O2、Ce 0.67 Zr 0.33 O2、Ce 0.75 Zr 0.25 O2 and Ce 0.8 Zr 0.2 O2.

[0047] Figure 1 The XRD spectra of samples with different Ce / Zr ratios obtained by the present invention are presented. It can be seen from the figure that no ZrO2 characteristic diffraction peak is observed in all samples, indicating that the prepared cerium-zirconium solid solution has a uniform and stable crystal phase structure. As the Ce / Zr ratio increases, the half-peak width of the diffraction peak of the cerium-zirconium solid solution gradually decreases, and 2θ shifts to a small angle direction. This is mainly due to the fact that Zr with a smaller ionic radius 4+ (0.084nm) into the CeO2 lattice (Ce 4+ 0.097nm), resulting in lattice distortion and lattice contraction. The results of calculating the half-peak width of the main peak at 29° and N2 adsorption and desorption show that as the Ce / Zr ratio increases, the grain size gradually increases and the specific surface area gradually decreases, indicating that Zr 4+ The introduction of inhibits particle aggregation during sample calcination and improves the material's high-temperature sintering resistance.

[0048] Figure 2 The Raman spectrum of the cerium-zirconium solid solution obtained by the present invention is presented. (a) Ce 0.2 Zr 0.8 O2,(b)Ce 0.33 Zr 0.67 O2,(c)Ce 0.67 Zr 0.33 O2,(d)Ce 0.75 Zr 0.25 O2, (e)Ce0.8 Zr 0.2 O2. It can be seen from the figure that with the increase of Zr content, the Raman spectrum changes significantly, indicating that the sample transforms from cubic phase to tetragonal phase. For the Raman spectrum of cubic phase, Figure (c), (d), (e), at ~470cm -1 There is a strong Raman vibration peak at the position, which is attributed to the F of O-Ce-O or O-Zr-O. 2g Symmetrical vibration. At ~600cm -1 There is a weak Raman vibration peak at , which is mainly attributed to the internal oxygen vacancies. 2g Vibration splits into B 1g and E g Vibration, Figure (a), (b), illustrates the transition of the material from cubic phase to tetragonal phase. 1g The vibration is the asymmetric vibration of MOM (M = Ce, Zr), and E g The vibration is the symmetric vibration of MOM (M = Ce, Zr). At the same time, at ~260cm -1 There is an obvious Raman vibration peak at the Zr-O-Zr 1g Symmetrical vibration.

[0049] Figure 3 The XPS spectra of (a) Ce 3d, (b) Zr 3d, and (c) O 1s of the cerium-zirconium solid solution obtained by the present invention are presented. As can be seen from the figure, the Ce 3d spectrum has ten peaks after peak fitting, corresponding to five pairs of spin-orbit coupling, indicating that Ce on the surface of the solid solution 3+ and Ce 4+ The peaks at 880.4, 882.6, 885.1, 889.3 and 898.4 eV are labeled v0, v, v′, v″ and v″′, respectively, and are attributed to Ce 3d 5 / 2 The peaks at 898.9, 901.1, 903.4, 908.0 and 916.9 eV are marked as u0, u, u′, u″ and u″′, respectively, and are attributed to Ce 3d 3 / 2 Characteristic peaks. v0, u0, v′ and u′ are derived from Ce 3+ species, while the six peaks of u, u″, u″′, v, v″′ and v′″ are all derived from Ce 4+ Species. According to the charge conservation principle, Ce on the surface of solid solution 3+ The presence of Ce on the surface of the material also indicates the presence of surface oxygen vacancies. 3+ The content of Zr increases first and then decreases with the increase of Ce / Zr ratio, and the number of oxygen vacancies on the surface of the material also shows the same trend. The Zr 3d spectrum has two peaks. The peak at 182.0 eV belongs to Zr 3d5 / 2 , the peak at 184.4 eV is attributed to Zr3d 3 / 2 These peaks are clearly identifiable without satellite peaks. The difference in binding energy between the two peaks is 2.4 eV, indicating that Zr in the sample exists in a +4 valence state. The O 1s curve after peak fitting has three peaks. The peak at a lower binding energy (~529.5 eV) (O I ) is attributed to the lattice oxygen in the solid solution. The shoulder peak (O II ) belongs to the adsorbed oxygen species (O - or –OH). O III (~531.8eV) corresponds to weakly bound surface oxygen species. The results show that the surface adsorbed oxygen also increases first and then decreases with the increase of Ce / Zr ratio. The presence of surface oxygen vacancies can adsorb more free oxygen.

[0050] Figure 4 The H2-TPR spectra of the cerium-zirconium solid solution obtained by the present invention are presented. From the H2-TPR spectra of samples with different Ce / Zr ratios before the cyclic reaction, it can be seen that the sample with a Ce / Zr ratio less than 1 (Ce 0.2 Zr 0.8 O2 and Ce 0.33 Zr 0.67 O2) has two reduction peaks, which are respectively attributed to the surface reduction peak at a lower temperature and the bulk reduction peak at a higher temperature. 0.67 Zr 0.33 O2、Ce 0.75 Zr 0.25 O2 and Ce 0.8 Zr 0.2 O2) only one main reduction peak was observed, and there was no obvious surface reduction peak and bulk reduction peak, indicating that Ce on the surface and in the bulk of the material 4+ As the Ce / Zr ratio increases, the reduction peak temperature shows a trend of first decreasing and then increasing, and the peak area first increases and then decreases, indicating that the reduction ability of the material first increases and then decreases as the Ce / Zr ratio increases.

[0051] Figure 5The TGA curves of the CO2 decomposition cyclic reaction of the cerium-zirconium solid solution with different Ce / Zr ratios before the cyclic reaction obtained by the implementation of the present invention are presented. Each sample was subjected to four cyclic reactions at normal pressure, and the reaction temperatures of the two steps were 1400°C and 1100°C, respectively. It can be seen that with the increase of temperature, the mass of all samples initially had an obvious decrease, which was mainly due to the decomposition of substances such as water and carbonates attached to the surface of the samples. Subsequently, a slow mass loss can be observed, indicating that the material begins a thermal reduction reaction. When CO2 is introduced at 1100°C, the mass of the material increases, indicating that the CO2 decomposition reaction is proceeding.

[0052] Figure 6 The average volume of CO and the average degree of reduction of samples with different Ce / Zr ratios obtained by the present invention are presented in the cyclic reaction. It can be seen that as the Ce / Zr ratio increases, the average volume of CO and the average degree of reduction increase first and then decrease. When the Ce / Zr ratio is equal to 1, the reaction catalytic activity is the best. The Ce / Zr ratio is 3:1, that is, Ce 0.75 Zr 0.25 O2 has the best cycle stability, and the CO production remains relatively stable during the three cycle reactions.

[0053] Figure 7 The average reduction degree of the cerium-zirconium solid solution material obtained by the present invention is shown in Figure 2. 3+ / Ce 4+ Molar ratio relationship diagram. In the cerium-zirconium solid solution, Zr doping will cause lattice distortion of CeO2, generate lattice defects, and produce more oxygen vacancies, which will enhance the mobility of bulk oxygen ions. When the Zr content gradually increases, the cerium-zirconium solid solution transforms from a cubic phase to a tetragonal phase. The migration ability of oxygen ions in different lattice structures is different. Since the mobility of oxygen ions in the cubic phase is higher than that in the tetragonal phase, the cubic phase is more conducive to the reduction of bulk CeO2 than the tetragonal phase. The XPS and H2-TPR results of the cerium-zirconium solid solution material before the cyclic reaction show that as the Ce / Zr ratio increases, the number of oxygen vacancies and the reduction performance first increase and then decrease. The more oxygen vacancies a material has, the stronger its oxygen storage and release capacity is, and the better the CO2 thermal decomposition reaction performance is.

[0054] In summary, the present invention obtains the following results: (i) As the Ce / Zr ratio increases, the crystal structure of the cerium-zirconium solid solution catalyst changes from a tetragonal phase to a cubic phase, the grain size decreases as the Zr content increases, and the specific surface area increases as the Zr content increases; (ii) As the Ce / Zr ratio increases, the number of oxygen vacancies and the reduction performance of the cerium-zirconium solid solution catalyst first increase and then decrease; (iii) In the two-step thermochemical CO2 decomposition reaction experiment, the catalytic activity of the cerium-zirconium solid solution catalyst first increases and then decreases as the Ce / Zr ratio increases, and the catalytic activity is best when Ce / Zr=1:1. In addition, all materials maintain good thermal stability and do not suffer from serious deactivation. Among them, Ce 0.75 Zr 0.25 O2 material has the best cyclic stability.

[0055] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.

Claims

1. Used to decompose CO 2 Preparation method of cerium-zirconium solid solution catalyst, steps include: Provide a P123 template; The template of P123, cerium salt and zirconium salt are mixed in a reaction solvent to obtain an intermediate product; The intermediate product is heat treated to obtain a cerium-zirconium solid solution catalyst.

2. The preparation method according to claim 1, It is characterized in that The method for preparing the P123 template comprises the following steps: P123 was stirred in anhydrous ethanol.

3. The preparation method according to claim 1, It is characterized in that The ratio of cerium salt, zirconium salt and P123 is: 80-160g P123 per 1mol of cerium salt and zirconium salt, preferably 90-130g P123, more preferably 100-120g P123.

4. The preparation method according to claim 1, It is characterized in that The cerium salt may be selected from Ce(NO 3 ) 3 、Ce 2 (SO 4 ) 3 、CeCl 3 One or more combinations of; and / or The cerium salt is provided in the form of a hydrate, an aqueous solution or an alcohol solution; and / or The zirconium salt may be selected from Zr(NO 3 ) 4 、Zr(SO 4 ) 2 、ZrCl 4 One or more combinations of; and / or The zirconium salt is provided in the form of its hydrate, aqueous solution or alcohol solution.

5. The preparation method according to claim 1, It is characterized in that The Ce / Zr ratio is 1:(0.1-5), more preferably 1:(0.15-4.5), more preferably 1:(0.2-4), such as 1:4, 1:3, 1:2, 2:1, 3:1, 4:

1.

6. The preparation method according to claim 1, It is characterized in that The P123, cerium salt and zirconium salt also evaporate the reaction solvent during the mixing process.

7. The preparation method according to claim 1, It is characterized in that The heat treatment is calcination, and the calcination temperature is 500-1000°C, more preferably 550-800°C, and more preferably 600-700°C.

8. The preparation method according to claim 7, It is characterized in that The calcination time is 1-8 hours, more preferably 2-6 hours, more preferably 4-5 hours.

9. The preparation method according to claim 7, It is characterized in that The heating rate of the calcination is 0.1-2°C / min, more preferably 0.2-1.5°C / min, more preferably 0.5-1°C / min.

10. A method for decomposing CO 2 Ce-Zr solid solution catalyst, It is characterized in that Obtained based on the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Catalyst for preparing carbon monoxide by decomposing carbon dioxide, as well as preparation method and application thereof

    CN103464134A

  • Catalyst used for thermochemical cyclic decomposition of CO2 and / or H2O and preparation method and application

    CN109317130A

  • Highly specific surface area possessed cerium-zirconium solid solution and its preparing method

    CN1565722A