Eggshell type hydrogenation catalyst, preparation method thereof and application of eggshell type hydrogenation catalyst in CBDK hydrogenation synthesis of CBDO

By adopting eggshell structure and tube-type isothermal reactor in CBDK hydrogenation catalyst, the problems of low catalyst activity and insufficient stability in the prior art are solved, and continuous production of CBDO with high selectivity and high yield is achieved .

CN118949978APending Publication Date: 2024-11-15ZHEJIANG HENGYI PETROCHEMICAL RES INST CO LTD

Patent Information

Application Number
CN202410992797.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing CBDK hydrogenation catalysts are low in activity and are prone to inactivation under high temperature conditions, and have low mass transfer and heat transfer efficiency, resulting in insufficient selectivity and stability of CBDO, making it difficult to achieve continuous production.

Method used

Eggshell hydrogenation catalyst is adopted, and its main active metal Ru and metal/oxide are enriched on the support surface to form a shell layer with a thickness of 5-100μm. Combined with the optimization process of the column tube isothermal reactor, it achieves a low hydrogen-oil ratio , high selectivity and high yield production under low thermal load.

Benefits of technology

It significantly improves the CBDK conversion rate and CBDO selectivity, extends the service life and stability of the catalyst, and realizes continuous and stable production of CBDO. The catalyst exhibits high selectivity and high yield under low hydrogen and oil ratio and low thermal load conditions. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949978A_ABST
    Figure CN118949978A_ABST
Patent Text Reader

Abstract

The invention relates to the field of chemical engineering, and discloses an eggshell type hydrogenation catalyst and a preparation method thereof, and application of the eggshell type hydrogenation catalyst in CBDK hydrogenation synthesis of CBDO. In the hydrogenation catalyst, the main active metal and the auxiliary metal / or oxides thereof are mainly enriched on the surface of the carrier to form an eggshell-shaped shell layer. Compared with a conventional hydrogenation catalyst for synthesizing CBDO through CBDK hydrogenation, the hydrogenation catalyst with the structural characteristics has the characteristics of high CBDK conversion rate, high CBDO selectivity, high stability after repeated use and long service life. By combining hydrogenation reaction process optimization and reactor optimization, high-selectivity and high-yield CBDO continuous production can be realized under the conditions of low hydrogen-oil ratio and low thermal load.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical industry, and in particular to an eggshell-type hydrogenation catalyst and a preparation method thereof, and application thereof in CBDK hydrogenation synthesis of CBDO. Background Art

[0002] 2,2,4,4-Tetramethyl-1,3-cyclobutanediol (CBDO) is an important aliphatic diol monomer for producing high-end copolyester products. It is mainly used to produce high-performance copolyester products with high transparency, high impact strength, high glass transition temperature and good toughness. It is green and environmentally friendly and is expected to replace traditional polycarbonate, with broad market prospects.

[0003] There are two main production processes for CBDO: a thermal cracking process using isobutyric acid or isobutyric anhydride as raw materials and a dehalogenation synthesis process using isobutyryl chloride as raw materials. Among them, the dechlorination process using isobutyryl chloride as raw material in CN103694083A has many synthetic by-products, large solvent usage, low yield and other problems, which do not meet the conditions for industrial production; while the thermal cracking process using isobutyric acid or isobutyric anhydride to produce CBDO has few by-products, high single-pass yield, and is easy to scale up. In the production process using isobutyric anhydride as raw material, isobutyric acid or isobutyric anhydride is first thermally cracked to produce dimethyl ethylene ketone (DMK); secondly, DMK is dimerized to obtain 2,2,4,4-tetramethyl-1,3-cyclobutanedione (CBDK); finally, CBDO is obtained by CBDK hydrogenation process. Among them, CBDK hydrogenation is the key to this process.

[0004] In recent years, the active metals of CBDK hydrogenation catalysts mainly include transition metals Ni, Co, Cu, and precious metals Pt, Pd, Ru, etc. Studies have found that the transition metal Ni, Co, and Cu-based catalysts reported in US9206950, US20080132737A1, US20080132738A1, US20080132739, US20080132742A1, A1CN105732329, and CN110124674A need to be at a higher temperature to ensure a certain catalytic activity. However, under high temperature conditions, CBDK is prone to ring-opening reactions to generate ring-opening byproducts such as 1-hydroxy-2,2,4-trimethyl-pentanone and 2,2,4-trimethyl-1,3-pentanediol, and the reaction thermodynamics is unfavorable.

[0005] US8420868B2 reported that Ru / carbon nanotube catalyst was used to carry out hydrogenation reaction of CBDK in a slurry bed reactor, with an operating temperature of 120°C and a pressure of 2.7 MPa. When CBDK was fully converted, the selectivity of CBDO was about 94%. Although the patent used a slurry bed reactor to carry out hydrogenation reaction of CBDK, which enhanced mass transfer and heat transfer, the full intermittent operation could not achieve continuous production of CBDO.

[0006] US20120149947A reported the CBDK hydrogenation reaction of Ru-based catalysts, the reactor used was a trickle bed hydrogenation reactor, the operating temperature was 130-160°C, the pressure was 1.4-2.1 MPa, the hydrogen-to-oil ratio was 150-600, and the selectivity of CBDO was 70-95% when CBDK was nearly completely converted. US20170334815A1 reported Ru / MAlO (M is an alkaline earth metal) catalyst, an adiabatic trickle bed hydrogenation reactor was used, the operating temperature was 80-135°C, the pressure was 2-6 MPa, the hydrogen-to-oil ratio was 69:1, and the selectivity of CBDO was 78-98% when CBDK was nearly completely converted. In the above patents, an adiabatic trickle bed reactor (trickle bed reactor) and a uniform particle catalyst were used, and the precious metal Ru loading was usually 2-10wt%. The hydrogen-to-oil ratio in this reactor is too high, and heat transfer is attempted to be achieved through hydrogen. The hydrogen phase is the continuous phase and the liquid CBDK solution is the dispersed phase, which is greatly affected by mass transfer. The CBDK hydrogenation reaction is a fast reaction and is greatly affected by the diffusion within the catalyst. When the trickle bed hydrogenation process is used, the uniform catalyst is more affected by mass and heat transfer, resulting in low utilization of the active components of the catalyst. Among them, the Ru loading of the optimal embodiment of US20120149947A is as high as 7%, and the Ru loading of the optimal embodiment of US20170334815A1 is as high as 8%, while the mass space velocity WHSV of the two is only 0.19 and 0.24h -1 , the annual CBDO production per unit catalyst is extremely low; at the same time, the hydrogenation of CBDK is a highly exothermic reaction and is extremely sensitive to temperature changes. The use of an adiabatic trickle bed hydrogenation reactor is not conducive to heat transfer. If improperly controlled, local hot spots will be generated in the catalyst bed, accelerating catalyst deactivation and reducing catalyst life. At present, there is no patent report on the stability of CBDK hydrogenation catalysts. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides an eggshell-type hydrogenation catalyst and a preparation method thereof, and an application thereof in the hydrogenation synthesis of CBDO by CBDK. The main active metal and auxiliary metal / or its oxide in the hydrogenation catalyst of the present invention are mainly enriched on the surface of the carrier to form an eggshell-shaped shell. Compared with the conventional hydrogenation catalyst used for the hydrogenation synthesis of CBDO by CBDK, the hydrogenation catalyst with this structural feature has the characteristics of high CBDK conversion rate, high CBDO selectivity, high stability after repeated use, and long service life. Combined with the optimization of the hydrogenation reaction process and the optimization of the reactor of the present invention, the continuous production of CBDO with high selectivity and high yield can be achieved under the conditions of low hydrogen-to-oil ratio and low heat load.

[0008] The specific technical scheme of the present invention is: In a first aspect, the present invention provides an eggshell-type hydrogenation catalyst in a granular form, comprising: a carrier, and a shell layer with a thickness of 5 to 100 μm and enriched on the surface of the carrier in an eggshell shape; the shell layer comprises a main active metal particle Ru and a co-metal and / or its oxide particles; wherein: The loading amount of the main active metal Ru is 0.5 to 1 wt% of the hydrogenation catalyst component; The auxiliary metal and / or its oxide particles are selected from Zn, Cu, Fe, Ce, Co, Sn, Ga, ZnO, CuO, Fe 2 O 3 、Ce 2 O 3 、Co 2 O 3 SnO 2 and Ga 2 O 3 At least one of the following: the molar ratio of Ru to the auxiliary metal and / or oxide is 0.1 to 1:1.

[0009] The hydrogenation catalyst of the present invention is characterized by being eggshell-shaped, that is, the main active metal and the auxiliary metal / or its oxide are mainly enriched on the surface of the carrier (the content inside the carrier is very low), forming an eggshell-shaped shell layer. The present invention finds that the hydrogenation catalyst with this structural feature can greatly reduce the influence of mass transfer on the catalyst performance compared with the conventional hydrogenation catalyst used for CBDK hydrogenation to synthesize CBDO, and has the characteristics of high CBDK conversion rate, high CBDO selectivity, high stability after repeated use, and long service life.

[0010] The present invention finds that the thickness of the shell has an important influence on the performance of the hydrogenation catalyst. If the shell thickness is too thin, the metal particles are easily agglomerated during calcination, resulting in the growth of the metal particle size, affecting the CBDK hydrogenation activity. At the same time, the anchoring degree of the metal particles on the surface of the catalyst carrier is not strong when the shell is too thin, and metal loss is likely to occur during the gas-liquid-solid three-phase reaction, causing irreversible deactivation of the catalyst. On the contrary, if the catalyst shell thickness is too thick, the catalyst will no longer be an eggshell distribution or the eggshell depth is too deep. Since the CBDK hydrogenation reaction is a fast reaction, the reaction is limited by mass transfer, and the catalyst eggshell thickness is too deep, which will cause the CBDK hydrogenation reaction rate to slow down, thereby affecting the catalytic activity and selectivity. At the same time, a higher metal loading is often required when the uniform type or eggshell depth is too deep, resulting in a low utilization rate of the catalyst precious metal. Preferably, the thickness of the shell is 10 to 50 μm.

[0011] The present invention finds that the calcination process directly affects the structure and performance of the catalyst. Specifically: if the oxygen content is too high, the carrier structure will be easily destroyed; if the oxygen content is too low, the calcination effect will be poor, and the strong interaction between the carrier and the metal cannot be effectively formed, resulting in easy loss of the catalyst and poor stability. In addition, the calcination rate should not be too fast, usually 1-2°C / min, to prevent the rapid temperature change from affecting the pore structure of the carrier. The calcination temperature is usually controlled at 100-350°C. The particle size of the metal particle Ru is 0.05-2nm; the particle size of the co-metal and / or its oxide particles is 0.05-2nm; the particle size of the eggshell-type hydrogenation catalyst is 0.5-3mm; the average pore size is 1.2-15nm; the pore volume is 0.05-1.5m 3 / g, specific surface area is 500~2000m 2 / g, mechanical strength 50-400N / cm 2 .

[0012] Preferably, the carrier is one or more of silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, diatomaceous earth, carbon nanotubes, activated carbon, molecular sieves, rare earth oxides, silicon carbide, organic metal frameworks and organic porous polymers.

[0013] Preferably, the particle size of the carrier is 0.5 to 3 mm, and the shape is one or more of clover-shaped, cylindrical, spherical, columnar and irregular.

[0014] Further preferably, the carrier is selected from alumina, activated carbon and molecular sieve; Still further preferably, the activated carbon is coconut shell carbon, wood carbon, petroleum-based carbon or asphalt-based carbon.

[0015] The key to the preparation of eggshell-type hydrogenation catalysts with the carrier of the present invention is that the carrier must be a shaped structure with certain mechanical strength and particle size, rather than a powder carrier. Since the particle size of the powder carrier is too low and the particles themselves are 1 to 50 μm, the bed pressure drop in the tube-type trickle bed reactor used for gas-liquid-solid three-phase is too high, and it is difficult to industrialize. It must be processed by mechanical molding. The mechanical strength after molding is too low. The molded structure is easy to collapse when loaded by a simple impregnation or stirring precipitation method. If the precious metal is loaded first and then molded, the prepared catalyst is usually a uniform catalyst rather than an eggshell-type hydrogenation catalyst. Therefore, compared with the traditional preparation method, the selection of the eggshell-type hydrogenation catalyst carrier of the present invention is mainly concerned with the mechanical strength, specific surface area, pore structure and surface properties of the molded carrier.

[0016] In the second aspect, the present invention provides a method for preparing the above-mentioned eggshell-type hydrogenation catalyst, comprising: immersing the carrier in a precursor solution containing Ru ions and auxiliary metal ions, first adjusting the pH to 0-5 for adsorption for 5-50 hours, then adjusting the pH to 8-12 for precipitation, washing and drying the precipitate, and calcining it in an atmosphere with an oxygen content of 3-5% for 1-5 hours, with a heating rate of 1-2°C / min and a calcination temperature of 100-350°C.

[0017] In the above preparation method, the present invention regulates the thickness of the shell by controlling the immersion adsorption time and the pH value of the adsorption and precipitation process. For the adsorption time: if the adsorption time is too short, the shell formed is too thin, which will not only lead to poor CBDO selectivity, but also cause the shell components to easily fall off from the carrier surface during the reaction, that is, the catalyst stability will be greatly reduced. If the adsorption time is too long, the shell formed is thicker. Although it has little effect on the catalyst stability, it is found that the CBDO selectivity is slightly reduced. For pH: the adsorption pH has a greater effect on the CBDO selectivity. If the pH is too high, Ru will be precipitated prematurely and cannot be effectively adsorbed by the carrier, resulting in a reduction in the loading amount.

[0018] Preferably, the Ru ions in the precursor solution exist in the form of ruthenium trichloride, ruthenium acetate and ruthenium acetylacetonate.

[0019] Preferably, the concentration of Ru ions in the precursor solution is 0.05-0.5 g / mL.

[0020] The present invention finds that the concentration of Ru in the precursor solution affects the activity of the catalyst. When the Ru concentration is too high or too low, the selectivity of CBDO will decrease. This is because the concentration of Ru during the loading process affects the speed of Ru adsorption in the activated carbon pores, the loading amount, and the particle size of the metal particles. Low loading amount or large metal particles will slow down the hydrogenation reaction rate of CBDO.

[0021] Preferably, the adsorption temperature is 20-95°C.

[0022] The adsorption temperature mainly affects the movement rate and adsorption rate of metal ions. The higher the adsorption temperature, the faster the molecules move and the deeper they move in the pores of the carrier. When the adsorption temperature is too high, the shell thickness is too thick and even an eggshell-type hydrogenation catalyst cannot be formed (when the metal particles penetrate into the pores inside the carrier, they are evenly distributed in the carrier rather than mainly enriched on the surface of the carrier), which ultimately affects the selectivity, yield and stability of CBDO.

[0023] Preferably, the precipitant used for the precipitation is ammonia water, urea, sodium hydroxide or sodium bicarbonate.

[0024] In a third aspect, the present invention provides the use of the eggshell-type hydrogenation catalyst in the hydrogenation synthesis of CBDO from CBDK.

[0025] In a fourth aspect, the present invention provides a method for synthesizing CBDO by hydrogenation of CBDK, comprising: hydrogen, CBDK and a hydrogenation solvent are mixed and preheated in a preheater, and introduced into a shell-and-tube isothermal reactor filled with the above-mentioned eggshell-type hydrogenation catalyst for hydrogenation reaction, the product is separated into gas and liquid, the obtained hydrogen is condensed to separate the entrained solvent and then reused, the obtained liquid is evaporated to recover the solvent and then crystallized to obtain CBDO.

[0026] The present invention uses a shell-and-tube isothermal reactor as a hydrogenation reactor for the first time. Compared with a conventional trickle bed reactor, the shell-and-tube isothermal reactor can meet the uniform distribution of the three phases of gas, liquid and solid, realize uniform and controllable temperature in the reaction bed, greatly reduce the hydrogen-to-oil ratio, and enable the hydrogenation catalyst to operate for a long period of time.

[0027] Preferably, the hydrogenation temperature is 80-130°C, the hydrogen / CBDK molar ratio (hydrogen-to-oil ratio) is 10-50:1, the reaction pressure is 2-4 MPa, and the volume space velocity is LHSV1-4N -1 , the feed concentration of CBDK is 5-25wt%.

[0028] The present invention finds that when the reaction temperature is too high and the liquid hourly space velocity is too low (the reaction residence time is too long), the CBDO selectivity decreases, mainly due to the increase in over-hydrogenation products. When the reaction temperature is too low, the catalyst has not yet been activated, and the low activity leads to a poor CBDO yield. When the hydrogen-to-oil ratio is too low, the CBDO selectivity is still high in the early stage, but as the temperature accumulates, local hot spots appear, and the CBDO selectivity gradually decreases. When the hydrogen-to-oil ratio is too high, the CBDO selectivity is high and the stability is good, but the bed pressure drop is significantly increased, which is beneficial to heat transfer but has high requirements on the mechanical strength of the catalyst, and the hydrogen cycle energy consumption is high. When the volumetric space velocity is large, the residence time is short, and the CBDK conversion rate and CBDO selectivity are both low.

[0029] Preferably, the hydrogenation solvent is selected from one or more of methanol, water, ethyl acetate, butyl acetate, butyl butyrate, isobutyl acetate and isopropanol.

[0030] Compared with the prior art, the beneficial effects of the present invention are: (1) The main active metal and auxiliary metal / or its oxide in the hydrogenation catalyst of the present invention are mainly enriched on the surface of the carrier to form an eggshell-like shell layer. Compared with the conventional hydrogenation catalyst used for hydrogenation of CBDK to synthesize CBDO, the hydrogenation catalyst with this structural feature has the characteristics of high CBDK conversion rate (more than 97%), high CBDO selectivity (more than 99%), high stability after repeated use (continuous stability evaluation time exceeds 8000 hours), and long service life.

[0031] (2) The present invention can ensure that a catalyst with an eggshell structure is obtained by optimizing the preparation process of the catalyst, and the shell thickness is adjusted within an ideal range, thereby further optimizing the conversion rate of the hydrogenation catalyst to CBDK, the selectivity to CBDO and the stability of the catalyst itself.

[0032] (3) Based on the eggshell-type hydrogenation catalyst of the present invention, combined with the optimization of the hydrogenation reaction process and the reactor type, high-selectivity and high-yield continuous stable production of CBDO can be achieved under low hydrogen-to-oil ratio and low heat load conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a high-resolution scanning electron microscope mapping image of the Ru-Zr / C hydrogenation catalyst prepared in Example 1.

[0034] Figure 2 This is a structural schematic diagram of the shell-and-tube isothermal reactor in Example 1.

[0035] Figure 3 This is a performance evaluation diagram of the CBDK hydrogenation stability of the hydrogenation catalyst prepared in Example 1.

[0036] The figures are marked as: gas-liquid separation zone 1, liquid collection zone 2, gas-liquid distributor 3, liquid distribution plate 4, liquid guide tube 5, medium inlet 6, reaction tube array 7, medium outlet 8, shell 9, gas-liquid outlet 10, gas-liquid inlet 11, support plate 12, baffle 13. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with the embodiments.

[0038] Overall embodiment An eggshell-type hydrogenation catalyst in a granular form comprises: an eggshell-type hydrogenation catalyst in a granular form comprises: a carrier, and a shell layer with a thickness of 5 to 100 μm and enriched on the surface of the carrier in an eggshell shape; the shell layer comprises main active metal particles Ru and auxiliary metal and / or oxide particles thereof; wherein: The loading amount of the main active metal Ru is 0.5 to 1 wt% of the hydrogenation catalyst component; The auxiliary metal and / or its oxide particles are selected from Zn, Cu, Fe, Ce, Co, Sn, Ga, ZnO, CuO, Fe 2 O 3 、Ce 2 O 3 、Co 2 O 3 SnO 2 and Ga 2 O 3At least one of the following: the molar ratio of Ru to the auxiliary metal and / or oxide is 0.1 to 1:1.

[0039] In some specific cases, the thickness of the shell layer is 10-50 μm; the particle size of the metal particles Ru is 0.05-2 nm; the particle size of the co-metal and / or its oxide particles is 0.05-2 nm; the particle size of the eggshell hydrogenation catalyst is 0.5-3 mm; the average pore size is 1.2-15 nm; the pore volume is 0.05-1.5 m 3 / g, specific surface area is 500~2000m 2 / g.

[0040] In some specific cases, the carrier is one or more of silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, diatomaceous earth, carbon nanotubes, activated carbon, molecular sieves, rare earth oxides, silicon carbide, organic metal frameworks and organic porous polymers.

[0041] In some specific cases, the particle size of the carrier is 0.5 to 3 mm, and the shape is one or more of clover, cylinder, sphere, column and irregular. Further preferably, the carrier is selected from alumina, activated carbon and molecular sieve; further preferably, the activated carbon is coconut shell carbon, wood carbon, petroleum-based carbon or asphalt-based carbon.

[0042] A method for preparing an eggshell type hydrogenation catalyst comprises: immersing a carrier in a precursor solution containing Ru ions and auxiliary metal ions, first adjusting the pH to 0-5 for adsorption for 5-50 hours, then adjusting the pH to 8-12 for precipitation, washing and drying the precipitate, and roasting it in an atmosphere with an oxygen content of 3-5% for 1-5 hours, with a heating rate of 1-2°C / min and a roasting temperature of 100-350°C.

[0043] In some specific cases, the Ru ions in the precursor solution exist in the form of ruthenium trichloride, ruthenium acetate and ruthenium acetylacetonate.

[0044] In some specific cases, the concentration of Ru ions in the precursor solution is 0.05-0.5 g / mL.

[0045] In some specific cases, the adsorption temperature is 20-95°C.

[0046] In some specific cases, the precipitating agent used for the precipitation is ammonia water, urea, sodium hydroxide or sodium bicarbonate.

[0047] A method for synthesizing CBDO by hydrogenation of CBDK comprises: hydrogen, CBDK and a hydrogenation solvent are mixed and preheated in a preheater, and introduced into a tubular isothermal reactor filled with an eggshell-type hydrogenation catalyst for hydrogenation reaction, the product is separated into gas and liquid, the obtained hydrogen is condensed to separate the entrained solvent and then reused, the obtained liquid is evaporated to recover the solvent and then crystallized to obtain CBDO.

[0048] In some specific cases, the hydrogenation temperature is 80-130°C, the hydrogen / CBDK molar ratio (hydrogen to oil ratio) is 10-50:1, the reaction pressure is 2-4 MPa, and the volumetric space velocity is LHSV1-4h -1 , the feed concentration of CBDK is 5-25wt%.

[0049] In some specific cases, the hydrogenation solvent is selected from one or more of methanol, water, ethyl acetate, butyl acetate, butyl butyrate, isobutyl acetate and isopropanol.

[0050] In some specific cases, the shell-and-tube isothermal reactor comprises: a shell 9, with gas-liquid inlet 11 and gas-liquid outlet 10 at both ends of the shell, and the inside of the shell is divided into gas-liquid separation zone 1, reaction zone and liquid collection zone 2 in sequence according to the gas-liquid inlet and gas-liquid outlet directions; a gas-liquid distributor 3 is provided at the gas-liquid inlet, the gas-liquid separation zone and the reaction zone are separated by a liquid distribution plate 4, and the liquid collection zone and the reaction zone are separated by a support plate 12; a plurality of parallel reaction tubes 7 are installed in the reaction zone, and the two ends of the reaction tubes are connected to the gas-liquid separation zone and the liquid collection zone through a liquid distribution plate and a support plate respectively; wherein the connection end of the reaction tube and the liquid distribution plate is a liquid guide tube 5 with a necking design. The gap between the reaction tubes in the reaction zone is a medium storage space, and a medium inlet 6 and a medium outlet 8 are provided at both ends of the reaction zone; a plurality of staggered baffles 13 are provided in the medium storage space. The eggshell-type hydrogenation catalyst is loaded in the reaction tube.

[0051] Unlike the traditional trickle bed reactor, the isothermal trickle bed reactor is a tube-in-tube type with multiple tube bundles, while the traditional trickle bed reactor is adiabatic and single tube. For reactions with small heat release and catalysts that are not sensitive to temperature, adiabatic trickle bed reactors are usually suitable, while the CBDK hydrogenation reaction has a large heat release and the catalyst is extremely sensitive to temperature, so a tube-in-tube isothermal reactor is used. Tube-in-tube reactors are usually used for gas-solid phase reactions and are rarely used in gas-liquid-solid three-phase reactions, mainly because it is difficult to distribute gas and liquid at the same time. In this scheme, the gas-liquid flow rate is not large, and the selection of a suitable gas-liquid distributor and reactor structure can achieve good distribution of gas and liquid.

[0052] In some specific cases, the gas-liquid distributor is a tube-type distributor, a nozzle-type distributor, a sieve plate-type distributor, a downcomer distributor and a bubble-cap distributor; a bubble-cap distributor is further preferred.

[0053] The gas-liquid distributor passes hydrogen into the reaction tubes through different gas-liquid flow rates, and the liquid flows into the reaction tubes through the liquid distribution plate and the liquid guide pipe. The eggshell type hydrogenation catalyst is loaded in the tube, and the shell layer is heat exchanged by heat transfer oil. The shell is equipped with baffles to make the liquid temperature evenly distributed. The heat released by the reaction is transferred by the heat transfer oil to ensure the uniform temperature in the reactor.

[0054] Specific Examples and Comparative Examples The CBDO stable operation time refers to the long-term operation time when the CBDK conversion rate is close to 100% and the CBDO selectivity is not less than 97%. In the embodiments and comparative examples, if the CBDO selectivity is less than 95%, the operation time is uniformly 200 hours.

[0055] Example 1 (I) Preparation of eggshell type RuZn / C hydrogenation catalyst, the specific steps are as follows: (1) Accurately weigh 2.23 kg of RuCl 3 , 1.85kg Zn(NO 3 ) 2 6H 2 O, using deionized water as solvent, to prepare 12L of Ru-Zn precursor solution. Then add 5kg of pre-dried shaped activated carbon, which is spherical with a particle size of about 1mm and is asphalt-based spherical activated carbon, adjust the pH value to 2.6 with dilute hydrochloric acid, and place in a heat-collecting constant temperature heating stirrer (40°C, 200rpm) to fully carry out ion adsorption for 48h to obtain a pre-liquid.

[0056] (2) Add a certain amount of dilute NaOH solution (concentration: 1 mol / L) to the pre-liquid obtained in step (1) using a microinjection pump. -1 ) until the initial pH value of the suspension is adjusted to 11, and the precipitation reaction is carried out in a heat-collecting constant temperature heating stirrer and stirred for 10 hours.

[0057] (3) The precipitate was filtered and washed with deionized water for three times, dried at 120° C. for 12 h, and calcined in a tubular high-temperature furnace in a low-oxygen atmosphere for 3 h. The oxygen content was controlled to 3.5%, the calcination temperature was 300° C., and the heating rate was 2° C. / min to obtain a Ru-Zn / C hydrogenation catalyst.

[0058] The quantitative results of ICP analysis showed that the loading amount of Ru was 0.95wt% and the loading amount of auxiliary metal Zn was 0.92wt%. 2 The specific surface area of ​​the catalyst measured by adsorption-desorption curve is 1360 g / cm 2 The average pore size of the catalyst is 1.2 nm and the pore volume is 1.05 m 3 / g. The catalyst was measured by scanning electron microscopy and was in the form of microspheres with a particle size of 0.8 mm. The catalyst density was measured to be 0.5 g / cm 3 HRTEM analysis of metal nanoparticles (Ru-Zn) showed an average particle size of 1.3 nm, and the metal Ru-Zn was mainly concentrated in the catalyst shell of the carrier with a thickness of about 15 μm. Figure 1 As shown, the catalyst is a typical eggshell type hydrogenation catalyst ( Figure 1 In the figure, A, a is a cross-sectional view; B, b is a stereoscopic view).

[0059] (ii) The Ru-Zn / CN hydrogenation catalyst prepared in step (1) is loaded into a shell-and-tube isothermal reactor. The structure of the shell-and-tube isothermal reactor is as follows: Figure 2 As shown, it includes: a shell 9, with gas-liquid inlet 11 and gas-liquid outlet 10 at both ends of the shell, and the inside of the shell is divided into gas-liquid separation zone 1, reaction zone and liquid collection zone 2 in sequence according to the gas-liquid inlet and gas-liquid outlet directions; a gas-liquid distributor 3 (bubble-type gas-liquid distributor) is provided at the gas-liquid inlet, the gas-liquid separation zone and the reaction zone are isolated by a liquid distribution plate 4, and the liquid collection zone and the reaction zone are isolated by a support plate 12; parallel reaction tubes 7 are installed in the reaction zone, and the two ends of the reaction tubes are connected to the gas-liquid separation zone and the liquid collection zone through the liquid distribution plate and the support plate respectively; wherein the connection end of the reaction tube and the liquid distribution plate is a liquid guide tube 5 with a necking design. The gap between the reaction tubes in the reaction zone is a medium storage space, and a medium inlet 6 and a medium outlet 8 are provided at both ends of the reaction zone; and a staggered baffle 13 is provided in the medium storage space. Eggshell-type hydrogenation catalyst is loaded in the reaction tube. Heat transfer oil is introduced into the medium storage space to remove the local heat release of the reaction to prevent the catalyst from being deactivated due to excessive local temperature rise.

[0060] (III) Hydrogen, CBDK and hydrogenation solvent are preheated to 100°C by a preheater, passed through a shell-and-tube isothermal reactor and continuously hydrogenated during the reaction. The CBDK hydrogenation temperature is controlled at 100°C, the hydrogen-oil ratio (hydrogen / CBDK molar ratio) is controlled at 30:1, the reaction pressure is controlled at 3Mpa, and the volumetric space velocity LHSV is controlled at 2h -1 , the feed mass concentration of CBDK is controlled to be 10wt%, and butyl acetate is selected as the hydrogenation solvent. The temperature distribution inside the bed is measured by a temperature sensor during the reaction process. The temperature inside the reactor is between 100-102°C. It can be seen that the temperature distribution inside the shell-and-tube isothermal reactor is uniform, and there is no local hot spot. The upper and lower outlet pressures in the reactor are 3.01Mpa and 2.99Mpa respectively, and the pressure drop inside the reaction tube is extremely low.

[0061] Through this industrial process, e.g. Figure 3As shown, the hydrogenation catalyst of the present invention can operate continuously and stably for more than 8000 hours, the conversion rate of CBDK is greater than 99.99%, the selectivity of CBDO is close to 99%, the stability of CBDO is good, and the yield of CBDO is high. After the reaction, the catalyst was subjected to ICP, BET, SEM and HRTEM characterization analysis. It can be seen that the catalyst particles are strong, there is no catalyst breakage in the SEM image, and the Ru content determined by ICP is still 0.98wt%, which is close to the Ru loading of the fresh catalyst. HRTEM image analysis shows that the particle size of the Ru metal particles is still 1.4±0.5nm, and the catalyst has no obvious sintering and growth phenomenon. In summary, it shows that the catalyst has excellent stability and has prospects for industrial application.

[0062] Example 2 The same eggshell-type RuZn / C hydrogenation catalyst raw material composition, the same shell-and-tube isothermal reactor and the same CBDK hydrogenation process as in Example 1 were used to explore the effect of the preparation method of the eggshell-type RuZn / C hydrogenation catalyst on the CBDK hydrogenation performance and stability.

[0063] Table 1: Effect of catalyst preparation process on CBDK hydrogenation performance From the data in Table 1, it can be seen that the preparation process of the catalyst has a great influence on the CBDK hydrogenation process, specifically: When the Ru precursor concentration is too high (Example 2-2) or too low (Example 2-1), the selectivity of CBDO is insufficient. This is because the concentration of Ru during the loading process affects the speed of Ru adsorption in the activated carbon pores, the loading amount, and the particle size of the metal particles. Low loading amount or large metal particles will slow down the hydrogenation reaction rate of CBDO.

[0064] Similarly, the adsorption time is 2 hours (Example 2-3), resulting in a slightly lower Ru loading amount. The thickness of Ru in the catalyst shell is too low, which makes the catalyst easy to fall off from the carrier surface during the reaction, resulting in a lower Ru loading amount after the reaction (i.e., poor catalyst stability) and poor CBDO selectivity. The adsorption time is 100 hours (Example 2-4). The long adsorption time mainly leads to a long catalyst loading time and high production cost. At the same time, the long adsorption time and the deep Ru loading thickness (within 100 μm) are still eggshell-type hydrogenation catalysts. The CBDO selectivity is slightly reduced, and the stability is not greatly affected.

[0065] The adsorption pH has a great influence on the selectivity of CBDO. Mainly, when the pH is too high (Example 2-5), the Ru metal is precipitated prematurely and cannot be effectively adsorbed in the pores of the carrier, and the loading amount is only 0.36%. When the pH value is appropriate, such as 1.8 (Example 2-6), the yield of CBDO is close to 99%, and the stability time exceeds 8000 hours.

[0066] The adsorption temperature mainly affects the movement rate and adsorption rate of metal ions. The higher the adsorption temperature, the faster the molecules move and the deeper they move in the carrier pores. For example, when the adsorption temperature is 90°C (Example 2-8), the Ru loading thickness is thicker (within 100 μm), but it is still an eggshell-type hydrogenation catalyst, the CBDO selectivity is about 97%, the main by-product is an intermediate product, and CBDO still has a good yield and stability.

[0067] Example 3 The same eggshell-type RuZr / C hydrogenation catalyst raw material composition and catalyst preparation process as in Example 1 and the same shell-and-tube isothermal reactor were used to investigate the effects of CBDK hydrogenation process conditions on the CBDK hydrogenation performance and stability.

[0068] Table 2: Effect of CBDK hydrogenation process conditions on hydrogenation performance From the data in Table 2, it can be seen that when the reaction temperature is too high (Example 3-2) and the liquid hourly space velocity is too low (Example 3-6) (the reaction residence time is too long), the CBDO selectivity decreases, mainly due to the increase in over-hydrogenation products. When the reaction temperature is too low (Example 3-3), the catalyst has not yet been activated, and the low activity leads to a poor CBDO yield. When the hydrogen-to-oil ratio is 5:1 (Example 3-4), the maximum bed temperature of the isothermal tube trickle bed reactor is still only 4.8°C, and the temperature is still within the preferred range. Therefore, the CBDO yield in the first 3000 hours is greater than 97%. However, as the temperature accumulates, local hot spots appear, and the CBDO selectivity gradually decreases to less than 97%. When the hydrogen-to-oil ratio is 100:1 (Example 3-5), the CBDO selectivity is close to 99%, and the stability is good, but the bed pressure drop is significantly increased. Although this is conducive to heat transfer, it has higher requirements on the mechanical strength of the catalyst and the hydrogen cycle energy consumption is high. When the volumetric space velocity is large, the residence time is short, and the CBDK conversion rate and CBDO selectivity are both low.

[0069] Example 4 The same eggshell-type RuZn / C hydrogenation catalyst raw material composition and catalyst preparation process and the same CBDK hydrogenation process as in Example 1 were used to explore the effects of the number of reaction tubes, the height-to-diameter ratio, and the gas-liquid distribution of the tube-in-tube isothermal reactor on the CBDK hydrogenation performance and stability.

[0070] Table 3: Effect of shell-and-tube isothermal reactor on CBDK hydrogenation performance It can be seen from the data in Table 3 that the gas-liquid distributor can use nozzle-type and sieve-plate-type distributors, and the selectivity and stability of CBDO are close to those in Example 1. The height-to-diameter ratio of the bed has a certain influence on the CBDK hydrogenation performance. When a certain amount of catalyst is met, the smaller the diameter of the single-tube reactor or the fewer the number of single-tube roots, the higher the reactor height, which is beneficial for temperature distribution, but unfavorable for pressure drop. In this embodiment, the gas velocity and liquid velocity are relatively small, less than 1 cm / s, and have little effect on the pressure drop, so the CBDO yield has little effect. However, when the diameter of the single tube becomes larger, the height-to-diameter ratio is too small or the number of single tube roots is too large, it may cause liquid bias or wall flow, which has a certain impact on the CBDO yield. When a heat transfer oil system is left in the shell, the maximum temperature rise of the reaction bed is about 2°C, indicating that the temperature control of the shell-and-tube isothermal reactor is better.

[0071] Comparative Example 1 The same tubular isothermal reactor and CBDK hydrogenation process conditions as in Example 1 were used. The catalysts used were 0.98% Ru-Zn / C and 5.67% Ru-Zn / C. Among them, 0.98% Ru-Zn / C was a homogeneous catalyst, not an eggshell type. The preparation method was as follows: accurately weigh 2.23 kg of RuCl 3 , 1.85kg Zn(NO 3 ) 2 6H 2 O, using deionized water as solvent, to prepare 12L of Ru-Zn precursor solution. Then add 5kg of pre-dried powdered activated carbon, the average particle size of which is about 20μm, which is wood powdered activated carbon. The pH value is adjusted to 2.6 by dilute hydrochloric acid, and placed in a heat-collecting constant temperature heating stirrer (40℃, 200rpm) for full ion adsorption for 48h to obtain a pre-liquid. A certain amount of dilute NaOH solution (concentration of 1mol L -1 ) until the initial pH value of the suspension is adjusted to 11, and the precipitation reaction is carried out in a heat-collecting constant temperature heating stirrer and stirred for 10 hours. The precipitate is filtered and washed with deionized water for 3 times, dried at 120°C for 12 hours, and calcined and activated in a tubular high-temperature furnace under a low oxygen content atmosphere for 3 hours, the oxygen content is controlled to 3.5%, the calcination temperature is 300°C, and the heating rate is 2°C / min to obtain a Ru-Zn / C hydrogenation catalyst. The obtained powdered Ru-Zn / C catalyst is used to obtain a granular uniform 0.98% Ru-Zn / C catalyst by tableting.

[0072] Table 4 Effect of distribution of active components of catalyst on hydrogenation performance It can be seen from the data in Table 4 that under the same experimental conditions, when the same loading amount of 0.98% as the eggshell type hydrogenation catalyst is used, the CBDO yield of the uniform catalyst is only 67.78%, while the CBDO yield of the uniform catalyst 5.67% Ru-Zn / C prepared with a high loading amount is 3% lower than that of the eggshell type hydrogenation catalyst, and the stability is also better, but the Ru utilization rate is low.

[0073] Comparative Example 2 The same eggshell-type RuZn / C hydrogenation catalyst raw material composition, catalyst preparation process, eggshell-type 0.98% Ru-Zn / C catalyst and CBDK hydrogenation process conditions as in Example 1 were used. The reactor form used was a common adiabatic trickle bed hydrogenation reactor, which was purchased from Shanghai Hanxing Energy Technology Co., Ltd., a DN200, 2m single-tube trickle bed adiabatic reactor.

[0074] Table 5: Effect of trickle bed reactor type on CBDK hydrogenation performance From the data in Table 5, it can be seen that the stability of the catalyst is relatively high within the first 2590 hours, but then the yield of CBDO continues to decrease. After 3500 hours, the CBDO selectivity is 56.87%. It can be seen that the CBDO yield of the adiabatic trickle bed hydrogenation reactor can meet the hydrogenation requirements when the initial activity is relatively high. As the reaction proceeds, the maximum temperature rise of the bed exceeds 29.8°C because the reaction heat cannot be removed in time. Especially when the hydrogen-to-oil ratio is low (when the hydrogen-to-oil ratio is 10:1), the maximum temperature rise of the bed exceeds 54.2°C, and the temperature has reached 180°C, which will cause the catalyst to sinter and deactivate rapidly. The CBDO selectivity is about 99% within the first 340 hours, and the CBDO selectivity decreases rapidly to 48.58% within 340 to 460 hours. When the hydrogen-to-oil ratio is 10:1 and the CBDK mass concentration is 20%, the stability of the CBDK hydrogenation catalyst is only maintained for 87 hours. Due to the rapid decrease in CBDO selectivity and the temperature rise of 78°C, the reactor is shut down. In addition, the adiabatic trickle bed has limited heat transfer means, and the only way to cool down the plant in industry is by stopping the plant or introducing cold hydrogen or cold nitrogen, which is not conducive to process stability. Therefore, the shell-and-tube isothermal reactor process system is suitable for large-scale industrial production to ensure the long-term stable operation of the catalyst.

[0075] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0076] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. An eggshell type hydrogenation catalyst, characterized in that: It is in granular form, comprising: a carrier, and a shell layer enriched on the surface of the carrier in an eggshell shape with a thickness of 5 to 100 μm; the shell layer comprises main active metal particles Ru and auxiliary metal and / or its oxide particles; wherein: The loading amount of the main active metal Ru is 0.5-1wt% of the hydrogenation catalytic component; The auxiliary metal and / or its oxide particles are selected from at least one of Zn, Cu, Fe, Ce, Co, Sn, Ga, ZnO, CuO, Fe2O3, Ce2O3, Co2O3, SnO2 and Ga2O3; the molar ratio of Ru to the auxiliary metal and / or oxide is 0.1~1:

1.

2. The hydrogenation catalyst according to claim 1, characterized in that: The thickness of the shell layer is 10-50 μm; The specific surface area of ​​the eggshell type hydrogenation catalyst is 500-2000m 2 / g; The particle size of the metal particles Ru is 0.05-2 nm; The particle size of the auxiliary metal and / or its oxide particles is 0.05-2 nm; The particle size of the eggshell type hydrogenation catalyst is 0.5-3 mm; the average pore size is 1.2-15 nm; the pore volume is 0.05-1.5 m 3 / g.

3. The hydrogenation catalyst according to claim 1 or 2, characterized in that: The carrier is one or more of silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, diatomaceous earth, carbon nanotubes, activated carbon, molecular sieves, rare earth oxides, silicon carbide, organic metal frameworks and organic porous polymers; The particle size of the carrier is 0.5-3 mm, and the shape is one or more of clover-shaped, cylindrical, spherical, columnar and irregular.

4. The hydrogenation catalyst according to claim 3, characterized in that: The carrier is alumina, activated carbon or molecular sieve.

5. The hydrogenation catalyst according to claim 4, characterized in that: The activated carbon is coconut shell carbon, wood carbon, petroleum-based carbon or asphalt-based carbon.

6. A method for preparing the eggshell-type hydrogenation catalyst according to any one of claims 1 to 5, characterized in that include: The carrier is immersed in a precursor solution containing Ru ions and auxiliary metal ions, the pH is first adjusted to 0-5 for adsorption for 5-50 hours, and then the pH is adjusted to 8-12 for precipitation. The precipitate is washed and dried, and calcined at 100-350°C at 1-2°C / min in an atmosphere with an oxygen content of 3-5% for 1-5 hours.

7. The preparation method according to claim 6, characterized in that: The Ru ions in the precursor solution exist in the form of ruthenium trichloride, ruthenium acetate and ruthenium acetylacetonate; The concentration of Ru ions in the precursor solution is 0.05-0.5 g / mL; The adsorption temperature is 20-95°C; The precipitating agent used for the precipitation is ammonia water, urea, sodium hydroxide or sodium bicarbonate.

8. Use of the eggshell-type hydrogenation catalyst according to any one of claims 1 to 5 or the eggshell-type hydrogenation catalyst obtained by the preparation method according to claim 6 or 7 in the hydrogenation synthesis of CBDO by CBDK.

9. A method for synthesizing CBDO by hydrogenation of CBDK, characterized in that include: Hydrogen, CBDK and a hydrogenation solvent are mixed and preheated in a preheater, and then introduced into a tubular isothermal reactor filled with the eggshell-type hydrogenation catalyst according to any one of claims 1 to 5 or the eggshell-type hydrogenation catalyst obtained by the preparation method according to claim 6 or 7 for hydrogenation reaction. The product is separated into gas and liquid, the obtained hydrogen is condensed to separate the entrained solvent and then reused, and the obtained liquid is evaporated to recover the solvent and then crystallized to obtain CBDO.

10. The preparation method according to claim 9, characterized in that: The hydrogenation temperature is 80-130°C, the hydrogen / CBDK molar ratio is 10-50:1, the reaction pressure is 2-4MPa, and the volume space velocity is LHSV1-4h -1 , CBDK feed concentration is 5-25wt%.

11. The preparation method according to claim 9, characterized in that: The hydrogenation solvent is selected from one or more of methanol, water, ethyl acetate, butyl acetate, butyl butyrate, isobutyl acetate and isopropanol.

Citation Information

Patent Citations

  • Production method of 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanediol

    CN112047813A

  • Noble metal-loaded eggshell type catalyst as well as preparation method and application thereof

    CN112264038A

  • Eggshell type Ru-based hydrogenation catalyst as well as preparation method and application thereof

    CN115155569A

  • Eggshell type catalyst, preparation method and application thereof, and method for preparing cyclohexane-1, 2-dicarboxylic acid diester through selective hydrogenation

    CN115709064A

  • Precious metal-loaded eggshell type catalyst, preparation method therefor, and application thereof

    WO2022099488A1

Cited By

  • Eggshell type gold catalyst and preparation method thereof

    CN120079374A