Nickel-iron alloy-based catalyst for preparing m-xylylenediamine through hydrogenation of isophthalonitrile and application of nickel-iron alloy-based catalyst

Through the combination of nickel-ferroalloy-based catalyst and transition metal and metal oxide support, combined with liquid ammonia solvent, the problem of polycondensation side reaction in the preparation of isophthalonitrile hydrogenation is solved, and high-efficiency and stable preparation of isophthalonitrile is achieved and the long life of the catalyst.

CN118949995APending Publication Date: 2024-11-15LANZHOU UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411005472.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Prior art Polycondensation side reactions are easily caused during the preparation of isophthalinium hydrogenation and isophthalinium. This leads to catalyst poisoning and inactivation, and it is difficult to effectively inhibit the generation of by-products, affecting product yield and catalyst life.

Method used

Using a nickel-ferroalloy-based catalyst, a high-activity, high selectivity and long-life catalyst is prepared by combining nickel-ferroalloy with transition metals such as Cu, Co, Sn, and metal oxide support such as TiO2, ZrO2, etc., and fixed. Liquid ammonia solvent is used in the bed reactor to inhibit polycondensation side reaction.

Benefits of technology

The efficient preparation of isophthalamine was achieved, the product yield reached 96.7%, and the catalyst was stable for more than 1,000 hours, which significantly improved the activity and life of the catalyst and reduced the generation of side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949995A_ABST
    Figure CN118949995A_ABST
Patent Text Reader

Abstract

The invention relates to a nickel-iron alloy-based catalyst for preparing m-xylylenediamine through hydrogenation of isophthalonitrile and application of the nickel-iron alloy-based catalyst, and relates to the technical field of catalysts. The catalyst used in the invention takes a nickel-iron alloy as an active component, or is doped with one or more of Cu, Co and Sn, and simultaneously takes a metal oxide, a composite metal oxide, activated carbon or diatomite as a carrier. The invention provides a method for synthesizing m-xylylenediamine, which comprises the following steps of: dissolving isophthalonitrile in liquid ammonia, adding a proper amount of organic solvent to prepare a raw material solution, and continuously carrying out hydrogenation reaction on the isophthalonitrile in a fixed bed reactor under the action of a nickel-iron alloy-based catalyst to realize high-activity and high-selectivity hydrogenation synthesis of the m-xylylenediamine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of m-phenylenediamine synthesis, specifically relating to a nickel-iron alloy catalyst for the hydrogenation of m-phenylenediamine by isophthalonitrile, a method for preparing the nickel-iron alloy catalyst, and a method for synthesizing m-phenylenediamine. Background Technology

[0002] m-Phenylenediamine (MXDA) is a high-performance epoxy resin curing agent with advantages such as low-temperature curing, heat resistance, water resistance, good chemical corrosion resistance, low viscosity, and easy operation. It can also be used in polyurethane, polyamide, rubber additives, fiber finishing agents, rust removers, chelating agents, lubricants, paper processing aids, and electronic chemicals. It is a widely used and high-value-added fine chemical.

[0003] Existing technologies primarily employ a process of catalytic hydrogenation of isophthalonitrile (IPN) to prepare m-phenylenediamine, typically using Raney Ni or Raney Co as the catalyst. This process is often carried out in a stirred tank batch operation. JP54-41804 discloses a method for preparing m-phenylenediamine using a Raney Ni or Raney Co catalyst and a mixed solvent of lower alcohols and aromatics. In a batch stirred tank, isophthalonitrile is hydrogenated to produce m-phenylenediamine; in the examples, the hydrogen pressure reaches as high as 11 MPa.

[0004] The hydrogenation reaction of isophthalonitrile produces highly reactive imine intermediates, which readily undergo further polycondensation reactions with intermediates and the target product, generating secondary amines, tertiary amines, and other high-boiling polymerization byproducts. These byproducts adsorb and deposit on the catalyst surface, often causing catalyst poisoning and deactivation. An important method to suppress polycondensation byproducts is to add excess liquid ammonia, ammonia gas, or organic amines as inhibitors. For example, CN101955432 discloses a method for the intermittent hydrogenation preparation of m-phenylenediamine in a stirred tank, using a modified Raney Ni catalyst, a ternary mixed solvent of aromatics, lower alcohols, and aliphatic halogenated derivatives, and secondary amine inhibitors such as triethylamine and diethylamine. CN102690205 discloses a process for preparing m-phenylenediamine by hydrogenation of isophthalonitrile under ammonia-conditioning. The process uses a Ni or Co catalyst supported on diatomaceous earth, activated carbon, alumina or silica, and with additives such as Re, Cu, Ru, and Fe. The process can completely convert isophthalonitrile in a trickle bed reactor, with a selectivity of up to 98.6% for m-phenylenediamine.

[0005] The yield of m-phenylenediamine can also be increased by adding promoters to the catalyst to improve catalytic activity and suppress side reactions. CN102029160 discloses a nickel catalyst supported on alumina, in which copper, cobalt, iron, zinc and other promoters are added, which can completely convert m-phenylenedionitrile under relatively mild conditions, with a selectivity of 98.8% for m-phenylenediamine. CN103539676 discloses a method for preparing m-phenylenediamine, which uses a nickel-based catalyst supported on alumina and adds molybdenum to the catalyst to suppress the formation of large molecular aggregates, thereby extending the catalyst lifetime.

[0006] In summary, the production of m-phenylenediamine using supported nickel-based catalysts and fixed-bed hydrogenation processes not only improves production efficiency and product yield but is also safe and environmentally friendly. Suppressing polycondensation side reactions is key to improving the yield of m-phenylenediamine, which requires not only the development of highly active, highly selective, and long-life hydrogenation catalysts but also improvements to the corresponding hydrogenation reaction processes. Summary of the Invention

[0007] To address the aforementioned technical problems, this invention provides a nickel-iron alloy-based catalyst for the catalytic hydrogenation of isophthalonitrile to m-phenylenediamine, a method for preparing the nickel-iron alloy-based catalyst, and a method for synthesizing m-phenylenediamine.

[0008] The nickel-iron alloy-based catalyst of the present invention is composed of an active component, a doped component, and a support;

[0009] The active component is a nickel-iron alloy; the doping component is a transition metal, which includes one or more of Cu, Co, and Sn.

[0010] The carrier is a metal oxide carrier, activated carbon, or diatomaceous earth.

[0011] The active component in the nickel-iron alloy-based catalyst has a mass content of 10-80 wt%;

[0012] The molar ratio of nickel to iron in the nickel-iron alloy is 5 to 10:1;

[0013] The mass content of the dopant component in the catalyst is 0-10 wt%.

[0014] The metal oxide support includes one or more of TiO2, ZrO2, MgO, Al2O3, CeO2 and ZnO.

[0015] The present invention also provides a method for preparing the nickel-iron alloy-based catalyst, which is an impregnation method, a co-precipitation method, or a deposition-precipitation method.

[0016] The impregnation method of the present invention includes the following steps:

[0017] S1: Dissolve the metal salts of Ni and Fe, or the metal salts of other transition metals Cu, Co, and Sn in water to prepare a metal salt solution, and add it to the carrier to mix and disperse evenly;

[0018] S2: Remove the solvent, dry the resulting solid, and then calcine it to obtain the nickel-iron alloy-based catalyst.

[0019] Furthermore, the concentration of the metal salt solution is 0.01–2 mol / L.

[0020] Furthermore, the stirring temperature is 30℃~90℃, and the stirring time is 2~24h.

[0021] Furthermore, the drying temperature is 60℃~300℃, the drying time is 4~24h, the calcination temperature is 200℃~800℃, preferably 300℃~600℃, and the calcination time is 2~24h, preferably 5~10h.

[0022] The co-precipitation method described in this invention includes the following steps:

[0023] S1: Dissolve the metal salts of Ni and Fe, or the metal salts of other transition metals Cu, Co, and Sn, in water to prepare a metal salt solution. Add the metal salt solution and the precipitant solution to a precipitation container for co-precipitation.

[0024] S2: The obtained precipitate is dried and then calcined to obtain a nickel-iron alloy-based catalyst.

[0025] Furthermore, the concentration of the metal salt solution is 0.01–2 mol / L.

[0026] Furthermore, the volume ratio of the metal salt solution to the precipitant solution is 1:1 to 10.

[0027] Furthermore, the coprecipitation temperature is 30℃~90℃, and the coprecipitation pH is 5~12.

[0028] Furthermore, the drying temperature is 60℃~300℃, the drying time is 4~24h, the calcination temperature is 200℃~800℃, preferably 300℃~600℃, and the calcination time is 2~24h, preferably 5~10h.

[0029] The deposition and precipitation method described in this invention includes the following steps:

[0030] S1: Dissolve the metal salts of Ni and Fe, or the metal salts of other transition metals Cu, Co, and Sn, in water to prepare a metal salt solution. Add a precipitant to precipitate the solution, and then add a carrier and stir to mix evenly.

[0031] S2. The obtained precipitate is dried and then calcined to obtain the composite metal oxide catalyst.

[0032] Furthermore, the concentration of the metal salt solution is 0.01–2 mol / L, and the concentration of the precipitant solution is 1–5 times the concentration of the metal salt aqueous solution.

[0033] Furthermore, the volume ratio of the metal salt solution to the precipitant solution is 1:1 to 10.

[0034] Furthermore, the coprecipitation temperature is 30℃~90℃, and the coprecipitation pH is 5~12.

[0035] Furthermore, the drying temperature is 60℃~300℃, the drying time is 4~24h, the calcination temperature is 200℃~800℃, and the calcination time is 2~24h.

[0036] The salt of the metal element is one or more of nitrates, sulfates, halides, and acetates.

[0037] The precipitant is one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium hydroxide, and potassium hydroxide.

[0038] Another object of the present invention is to provide the application of the nickel-iron alloy-based catalyst in the catalytic hydrogenation of isophthalonitrile to m-phenylenediamine. The method uses a fixed-bed reactor, in which isophthalonitrile is dissolved in liquid ammonia and an appropriate amount of organic solvent is added to prepare a feed solution. Under the action of the nickel-iron alloy-based catalyst, the feed solution reacts with hydrogen gas, thereby efficiently producing m-phenylenediamine.

[0039] Furthermore, the reaction conditions for the catalytic hydrogenation of isophthalonitrile to produce isophthalic dimethylamine are: temperature 60–200℃, pressure 1–25 MPa, and isophthalonitrile space velocity 0.1–2.0 h⁻¹. -1 The molar ratio of isophthalonitrile to hydrogen is 1:200, preferably 1:100.

[0040] Furthermore, the solvent in the isophthalonitrile feed solution is liquid ammonia and toluene, wherein the molar ratio of isophthalonitrile:toluene:liquid ammonia is 1:1:8 to 1:10:25.

[0041] Furthermore, before the reaction with hydrogen, the catalyst needs to be activated in situ. The temperature of the fixed bed reactor is raised to 300°C to 800°C at a heating rate of 1 to 10°C / min and held for 1 to 10 hours, and then cooled to the reaction temperature of 60 to 100°C.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] This invention provides a nickel-iron alloy-based catalyst for the hydrogenation of isophthalonitrile to prepare m-phenylenediamine. The active component is a nickel-iron alloy or a catalyst doped with one or more metals such as Cu, Co, and Sn, which is then supported on materials such as metal oxides, composite metal oxides, activated carbon, or diatomaceous earth. This invention also provides a fixed-bed catalytic hydrogenation method for isophthalonitrile to prepare m-phenylenediamine. Dissolving isophthalonitrile in liquid ammonia effectively suppresses the occurrence of condensation polymerization side reactions, thus improving the yield of the target product. The catalyst is adapted to its main reaction, enhancing the adsorption of unsaturated compounds such as imines while reducing the activity and number of adsorbed hydrogens, thereby increasing the yield of the product m-phenylenediamine.

[0044] The nickel-iron alloy catalyst of this invention can be used in the hydrogenation reaction of isophthalonitrile to produce m-phenylenediamine. The reaction is carried out under the following conditions: temperature 60–200°C, pressure 5–20 MPa, and isophthalonitrile space velocity 0.1–2.0 h⁻¹. -1 The yield of m-phenylenediamine can reach 96.7%. Furthermore, gas chromatography-mass spectrometry analysis shows that the nickel-iron alloy can operate stably for over 1000 hours.

[0045] The catalyst of this invention can be used for the hydrogenation reaction of isophthalonitrile to produce m-phenylenediamine. Under the following reaction conditions: temperature 60 to 200°C, pressure 5 to 20 MPa, and space velocity of isophthalonitrile 0.1 to 2.0 h⁻¹, a yield of m-phenylenediamine of 96.7% can be achieved. Furthermore, gas chromatography-mass spectrometry (GC-MS) analysis shows that the catalyst can operate stably for more than 1000 hours. Attached Figure Description

[0046] Figure 1 This is a stability test diagram of the hydrogenation of isophthalonitrile to produce isophthalic dimethylamine provided by the present invention. Detailed Implementation

[0047] The present invention will be further described below with reference to specific embodiments.

[0048] Example 1

[0049] Catalyst preparation by impregnation method: Mg1Al9O x As a catalyst support (where the molar ratio of Mg to Al is 1:9), 5g of Mg1Al9O xThe sample was added to a container containing 200 mL of deionized water and dispersed evenly. 10.41 g of Ni(NO3)2·6H2O and 6.51 g of Fe(NO3)3·9H2O were weighed and added to the mixture, and stirred at room temperature for 24 h. The elements were directly deposited onto a support by drying, and then calcined at 500 °C for 4 h to obtain a powder sample. An appropriate amount of the powder sample was placed in a mold and pressed into tablets, then sieved into 20–40 mesh granules and packed into a reduction tube. Reduction was carried out at 400 °C for 3 h under a 5% (v / v) H2 / Ar atmosphere, followed by passivation at a 1% (v / v) O2 / Ar atmosphere for 30 min, yielding a 60 wt% Ni7Fe3 / Mg1Al9O catalyst. x .

[0050] Synthesis of m-phenylenediamine: After adding isophthalonitrile and toluene solvent to the feed tank, the tank is sealed and then filled with argon gas. Argon gas is used to purge the tank three times to ensure an oxygen-free environment. Then, liquid ammonia is added, with a molar ratio of isophthalonitrile:toluene:liquid ammonia of 1:1:8. After the liquid ammonia is fully added, the system pressure is increased to 6 MPa, and the tank is shaken thoroughly to mix the feed. A fixed-bed reactor is used, and hydrogen is introduced to activate the catalyst in situ. The temperature of the fixed-bed reactor is increased to 500°C at a heating rate of 5°C / min and maintained for 2 hours, after which the temperature is lowered to the reaction temperature of 60°C. The feed solution is pumped into the bed containing the catalyst, and the reaction is carried out at a temperature of 60°C, a pressure of 7 MPa, and a m-phenylenediamine space velocity of 0.5 h⁻¹. -1 Under certain conditions, it reacts with hydrogen to produce m-phenylenediamine.

[0051] For ease of comparison, the composition of the catalysts, preparation methods, and reaction results are listed in Table 1.

[0052] Example 2

[0053] Catalyst preparation by coprecipitation: Ni, Fe, Mg, and Al metal nitrates were dissolved in a specific ratio, and a precipitant was added dropwise. Specifically, 10.41 g of Ni(NO3)2·6H2O, 6.51 g of Fe(NO3)3·9H2O, 2.11 g of Mg(NO3)2·6H2O, and 27.78 g of Al(NO3)3·9H2O were weighed into a container, and 500 mL of deionized water was added and stirred until homogeneous. Then, 1.5 mol / L Na2CO3 solution was added dropwise, controlling the pH of the system to 7–8. After the addition was complete, the mixture was stirred and dispersed for 2 hours, then transferred to an oil bath and aged at 80°C for 10 hours. After cooling to room temperature, the mixture was filtered and washed with deionized water until the pH of the filtrate reached 7. The resulting filter cake was dried, pulverized, and calcined in a muffle furnace at 400°C for 4 hours to obtain a powdered sample. The catalyst was pressed into tablets at 30 MPa, granulated, and sieved into 20–40 mesh particles. These particles were then packed into reduction tubes and reduced at 400 °C for 3 h under a 5% (v / v) H₂ / Ar atmosphere. Passivation was then performed for 10 min under a 1% (v / v) O₂ / Ar atmosphere to obtain a catalyst of 60 wt% Ni₇Fe₃ / Mg₁Al₉O₂. x .

[0054] The steps for synthesizing m-phenylenediamine are the same as in Example 1.

[0055] Example 3

[0056] Catalyst preparation by deposition-precipitation method: Specifically, 5g of Mg1Al9O x Disperse the solution evenly in a container containing 200 mL of deionized water. Weigh out 10.41 g of Ni(NO3)2·6H2O and 6.51 g of Fe(NO3)3·9H2O, add them to the solution, and stir to disperse evenly. Then, add 1.5 mol / L Na2CO3 solution dropwise, controlling the pH of the solution system to 7–8. After the addition is complete, stir and disperse for 2 hours, then transfer to an oil bath and age at 80°C for 10 hours. After the temperature dropped to room temperature, the mixture was filtered and washed with deionized water until the pH of the filtrate was 7. The resulting filter cake was dried and pulverized, then calcined in a muffle furnace at 400℃ for 4 hours to obtain a powder sample. This powder was then pressed into tablets at 30 MPa, granulated, and sieved into 20-40 mesh particles. The particles were then packed into a reduction tube and reduced at 400℃ for 3 hours under a 5% (v / v) H2 / Ar atmosphere. After switching to a 1% (v / v) O2 / Ar atmosphere, the mixture was passivated for 10 minutes to obtain a catalyst of 60wt% Ni7Fe3 / Mg1Al9O. x .

[0057] The steps for synthesizing m-phenylenediamine are the same as in Example 1.

[0058] Example 4

[0059] Catalyst preparation by coprecipitation: Similar to Example 2, except for the calcination process. Specifically, 11.89 g of Ni(NO3)2·6H2O, 4.34 g of Fe(NO3)3·9H2O, 2.11 g of Mg(NO3)2·6H2O, and 27.78 g of Al(NO3)3·9H2O were weighed into a container, and 500 mL of deionized water was added and stirred until dissolved. Then, an equivalent amount of Na2CO3 aqueous solution was added dropwise, controlling the pH of the system to 7–8. After the addition was complete, the mixture was stirred and dispersed for 2 hours, then transferred to an oil bath and aged at 80°C for 10 hours. After the temperature cooled to room temperature, the mixture was filtered and washed with deionized water until the pH of the filtrate was 7. The resulting filter cake was dried, pulverized, and transferred to a crucible. It was then calcined in a muffle furnace at 100°C for 2 hours, and then the temperature was increased to 400°C at a rate of 5°C / min and calcined for another 4 hours to obtain a powdered sample. The catalyst was pressed into tablets at 30 MPa, granulated, and sieved into 20–40 mesh particles. These particles were then packed into reduction tubes and reduced at 400 °C for 3 h under a 5% (v / v) H₂ / Ar atmosphere. Passivation was then performed for 10 min under a 1% (v / v) O₂ / Ar atmosphere to obtain a catalyst of 60 wt% Ni₈Fe₂ / Mg₁Al₉O₂. x .

[0060] The steps for synthesizing m-phenylenediamine are the same as in Example 1.

[0061] Example 5

[0062] Referring to Example 4, the difference lies in the relative contents of Ni and Fe; a 60wt% Ni9Fe1 / Mg1Al9O3 solution was prepared using a co-precipitation method. x Specifically, 13.38g of Ni(NO3)2·6H2O, 2.17g of Fe(NO3)3·9H2O, 2.11g of Mg(NO3)2·6H2O, and 27.78g of Al(NO3)3·9H2O were weighed into a container, and the subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 4.

[0063] Example 6

[0064] Referring to Example 4, the difference lies in the relative content of each component of the catalyst and the support. A co-precipitation method was used to prepare 10wt% Ni9Fe1 / Al2O3. Specifically, 2.23g of Ni(NO3)2·6H2O, 0.36g of Fe(NO3)3·9H2O, and 69.45g of Al(NO3)3·9H2O were weighed into a container. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 4.

[0065] Example 7

[0066] Referring to Example 3, the difference lies in the relative content of each component of the catalyst and the support. A 20wt% Ni8Fe2 / TiO2 was prepared using a deposition precipitation method. Specifically, 5g of commercial TiO2 was added to a container containing 200mL of deionized water and dispersed evenly. Then, 3.96g of Ni(NO3)2·6H2O and 1.45g of Fe(NO3)3·9H2O were weighed and added to the mixture, and stirred until evenly dispersed. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0067] Example 8

[0068] Referring to Example 3, the difference lies in the relative content of each component of the catalyst and the support. A 30wt% Ni7Fe3 / ZrO2 was prepared using a deposition precipitation method. Specifically, 5g of ZrO2 was added to a container containing 200mL of deionized water and dispersed evenly. Then, 5.20g of Ni(NO3)2·6H2O and 3.26g of Fe(NO3)3·9H2O were weighed and added to the mixture, and stirred until evenly dispersed. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0069] Example 9

[0070] Referring to Example 3, the difference lies in the relative content of the catalyst components and the support. A 40wt% Ni6Fe4 / MgO was prepared using a deposition-precipitation method. Specifically, 5g of laboratory-prepared MgO was added to a container containing 200mL of deionized water and dispersed evenly. Then, 5.95g of Ni(NO3)2·6H2O and 5.79g of Fe(NO3)3·9H2O were weighed and added to the mixture, and stirred until evenly dispersed. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0071] Example 10

[0072] Referring to Example 3, the difference lies in the relative content of the catalyst components and the support. 50wt% Ni9Fe1 / Al2O3 was prepared using a deposition precipitation method. 5g of laboratory-prepared γ-Al2O3 was added to a container containing 200mL of deionized water and dispersed evenly. 11.15g of Ni(NO3)2·6H2O and 1.81g of Fe(NO3)3·9H2O were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0073] Example 11

[0074] Referring to Example 3, the difference lies in the catalyst support; 60wt% Ni8Fe2 / SiO2 was prepared using a deposition-precipitation method. 5g of commercially available fumed SiO2 was added to a container containing 200mL of deionized water and dispersed evenly. 11.89g of Ni(NO3)2·6H2O and 4.34g of Fe(NO3)3·9H2O were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0075] Example 12

[0076] Referring to Example 3, the difference lies in the catalyst support; 70wt% Ni7Fe3 / activated carbon was prepared using a deposition-precipitation method. First, the activated carbon was pretreated. 10g of commercially available activated carbon was weighed into a three-necked flask, and 45g of a mixed acidic reagent prepared from 90% concentrated sulfuric acid, potassium persulfate, and potassium nitrate in a mass ratio of 38:3:1 was added. The mixture was slowly stirred, heated to 240℃ and maintained for 1.5h, then moderately cooled, and the acidic solution was recovered by filtration. The activated carbon was repeatedly washed with hot water until neutral, dried under vacuum, and then dried at 140℃ for 1 hour for later use. 5g of the treated activated carbon was added to a container containing 200mL of deionized water and dispersed evenly. 12.14g of Ni(NO3)2·6H2O and 7.60g of Fe(NO3)3·9H2O were weighed and added to the mixture, and stirred until evenly dispersed. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0077] Example 13

[0078] Referring to Example 3, the difference lies in the catalyst support; 80wt% Ni7Fe3 / diatomaceous earth was prepared using a deposition-precipitation method. 5g of commercially available diatomaceous earth was ground and added to a container containing 200mL of deionized water, where it was dispersed evenly. 13.87g of Ni(NO3)2·6H2O and 8.68g of Fe(NO3)3·9H2O were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0079] Example 14

[0080] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition; 70wt% Ni9Fe1 / ZnZrO was prepared using a deposition-precipitation method. x 5g of laboratory-made ZnZrO xAs a catalyst support (with a molar ratio of Zn to Zr of 1:1), it was added to a container containing 200 mL of deionized water and dispersed evenly. 15.61 g of Ni(NO3)2·6H2O and 2.53 g of Fe(NO3)3·9H2O were weighed and added to the container and stirred to disperse evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0081] Example 15

[0082] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition. A 60wt% Ni8Fe2 / CeO2 was prepared using a deposition precipitation method. Five laboratory-prepared CeO2 was added to a container containing 200mL of deionized water and dispersed evenly. 11.89g of Ni(NO3)2·6H2O, 4.34g of Fe(NO3)3·9H2O, and 1.14g of Cu(NO3)2·6H2O were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0083] Example 16

[0084] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition. A 50wt% Ni7Fe3 / ZnO catalyst was prepared using a deposition-precipitation method. 5g of laboratory-prepared ZnO was added to a container containing 200mL of deionized water and dispersed evenly. 8.67g of Ni(NO3)2·6H2O and 5.43g of Fe(NO3)3·9H2O were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0085] Example 17

[0086] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition. A 60wt% Ni6Fe3Cu1 / Al2O3 catalyst was prepared using a deposition-precipitation method. 5g of laboratory-prepared Al2O3 was added to a container containing 200mL of deionized water and dispersed evenly. 8.92g of Ni(NO3)2·6H2O, 6.51g of Fe(NO3)3·9H2O, and 1.14g of Cu(NO3)2·6H2O were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0087] Example 18

[0088] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition. A 60wt% Ni6Fe3Co1 / Al2O3 catalyst was prepared using a deposition-precipitation method. 5g of laboratory-prepared Al2O3 was added to a container containing 200mL of deionized water and dispersed evenly. 8.92g of Ni(NO3)2·6H2O, 6.51g of Fe(NO3)3·9H2O, and 1.37g of Co(NO3)2·6H2O were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0089] Example 19

[0090] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition. A 40wt% Ni8Fe1Co1 / TiO2 catalyst was prepared using a deposition precipitation method. 5g of commercially available TiO2 was added to a container containing 200mL of deionized water and dispersed evenly. 7.93g of Ni(NO3)2·6H2O, 1.45g of Fe(NO3)3·9H2O, and 0.91g of Co(NO3)2·6H2O were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0091] Example 20

[0092] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition. A 60wt% Ni6Fe3Co1 / ZnO catalyst was prepared using a deposition precipitation method. Five tons of laboratory-prepared ZnO were added to a container containing 200 mL of deionized water and dispersed evenly. 1.49 g of Ni(NO3)2·6H2O, 6.51 g of Fe(NO3)3·9H2O, and 1.23 g of SnCl4 were weighed and added to the mixture, then stirred and dispersed evenly. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0093] Comparative Example 1

[0094] Referring to Example 4, the difference is that the metal component contains only Ni, and 60wt% Ni / Mg1Al9Ox is prepared by co-precipitation. Specifically, 8.92g of Ni(NO3)2·6H2O, 2.11g of Mg(NO3)2·6H2O, and 27.78g of Al(NO3)3·9H2O are weighed into a container, and the subsequent catalyst preparation process and catalyst evaluation steps are the same as in Example 4.

[0095] Comparative Example 2

[0096] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition. A 70wt% Ni9Cu1 / TiO2 catalyst was prepared using a deposition precipitation method. 5TiO2 was added to a container containing 200mL of deionized water and dispersed evenly. 15.61g of Ni(NO3)2·6H2O and 1.33g of Cu(NO3)2·6H2O were weighed and added to the mixture, and stirred until evenly dispersed. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0097] Comparative Example 3

[0098] Referring to Example 3, the difference lies in the active metal and support in the catalyst composition. A 70wt% Ni9Co1 / SiO2 catalyst was prepared using a deposition precipitation method. 5SiO2 was added to a container containing 200mL of deionized water and dispersed evenly. 15.61g of Ni(NO3)2·6H2O and 1.60g of Co(NO3)2·6H2O were weighed and added to the mixture, and stirred until evenly dispersed. The subsequent catalyst preparation process and catalyst evaluation steps were the same as in Example 3.

[0099] Comparative Example 4

[0100] The catalyst is the same as in Example 4, which is 60 wt% Ni7Fe3 / Mg1Al9O prepared by co-precipitation. x The difference lies in the preparation of the raw material solution during the synthesis of m-phenylenediamine. Specifically, after adding isophthalonitrile and toluene to the raw material tank, the tank is sealed and then filled with argon gas. Argon gas is used to purge the tank three times to ensure that there is no oxygen in the tank. The molar ratio of isophthalonitrile to toluene in the raw material solution is 1:1. The subsequent steps for the synthesis of m-phenylenediamine are the same as in Example 1.

[0101] Comparative Example 5

[0102] The catalyst is the same as in Example 4, which is 60 wt% Ni7Fe3 / Mg1Al9O prepared by co-precipitation. x The difference lies in the preparation of the raw material solution during the synthesis of m-phenylenediamine. Specifically, after adding isophthalonitrile and liquid ammonia to the raw material tank, the tank is sealed and then filled with argon gas. Argon gas is used to purge the tank three times to ensure that there is no oxygen in the tank. The molar ratio of isophthalonitrile to liquid ammonia in the raw material solution is 1:10. The subsequent steps for the synthesis of m-phenylenediamine are the same as in Implementation 1.

[0103] For ease of comparison, the catalysts prepared in Examples 1-20 and Comparative Examples 1-5 above, as well as the results of the synthesis reaction of m-phenylenediamine, are listed in Table 1.

[0104] Table 1. Composition of the catalyst, preparation process, and results of the m-phenylenediamine synthesis reaction.

[0105]

[0106]

[0107] Note: *Other products mainly include high-boiling-point polymers.

[0108] Effect Analysis:

[0109] The following conclusions can be drawn from Table 1:

[0110] (1) In terms of the selection of active metal for catalyst, compared with single metal, the catalytic activity of nickel-iron alloy as active component is significantly improved, which indicates that nickel-iron alloy catalyst has a significant promoting effect in the reaction process of catalytic hydrogenation of isophthalonitrile to prepare isophthalic dimethylamine.

[0111] (2) Regarding the catalyst support, basic MgO was introduced into the composite oxide support, and the catalyst was prepared by deposition precipitation, which reduced the acidity of the catalyst. The present invention effectively suppressed the formation of condensation polymers. Compared with single oxides, the conversion rate of isophthalonitrile and the selectivity of the target product m-phenylenediamine were improved, and the yield was significantly increased.

[0112] (3) Using liquid ammonia as a solvent to prepare the raw material solution effectively suppressed the occurrence of polycondensation side reactions, and the yield of the target product m-phenylenediamine was significantly improved.

[0113] This invention also provides stability test results for the catalyst prepared in Example 1 used in the hydrogenation of isophthalonitrile to m-phenylenediamine (reaction conditions: temperature 60°C, pressure 7 MPa, liquid hourly space velocity of isophthalonitrile 0.5 h⁻¹). -1 The result is as follows Figure 1 As shown.

[0114] Effect analysis: The catalyst prepared by this invention can operate stably for more than 1000 hours under the reaction conditions without significant deactivation, which meets the requirements for industrial catalytic applications.

[0115] It should be noted that the above examples are merely some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments and other modifications are possible. All modifications directly or indirectly derived by those skilled in the art from the disclosure of the present invention should be considered within the scope of protection of the present invention.

Claims

1. A nickel-iron alloy-based catalyst for hydrogenating isophthalonitrile to produce meta-xylylenediamine, characterized in that: The nickel-iron alloy-based catalyst consists of an active component, a doping component and a carrier; The active component is a nickel-iron alloy; the doping component is a transition metal, and the transition metal includes one or more of Cu, Co, and Sn; The carrier is a metal oxide carrier, activated carbon or diatomaceous earth; The mass content of the active component in the nickel-iron alloy-based catalyst is 10 to 80 wt %; The molar ratio of nickel to iron in the nickel-iron alloy is 5 to 10:1; The mass content of the doping component in the catalyst is 0 to 10 wt%; The metal oxide carrier includes one or more of TiO2, ZrO2, MgO, Al2O3, CeO2 and ZnO.

2. A nickel-iron alloy-based catalyst for hydrogenating isophthalonitrile to meta-xylylenediamine according to claim 1, characterized in that: The preparation method of the nickel-iron alloy-based catalyst is an impregnation method, a co-precipitation method or a deposition precipitation method.

3. A nickel-iron alloy-based catalyst for hydrogenating isophthalonitrile to meta-xylylenediamine according to claim 2, characterized in that: The impregnation method The following steps are involved: S1: dissolving metal salts of Ni and Fe or metal salts of other transition metals Cu, Co, Sn in water to prepare a metal salt solution, adding the carrier to mix and disperse evenly; S2: removing the solvent, drying and calcining the obtained solid to obtain a nickel-iron alloy-based catalyst.

4. A nickel-iron alloy-based catalyst for hydrogenating isophthalonitrile to meta-xylylenediamine according to claim 2, characterized in that: The coprecipitation method comprises the following steps: S1: dissolving metal salts of Ni and Fe or metal salts of other transition metals Cu, Co, Sn in water to prepare a metal salt solution, and adding the metal salt solution and a precipitant solution into a precipitation container at the same time for co-precipitation; S2: The obtained precipitate is dried and then calcined to obtain a nickel-iron alloy-based catalyst.

5. A nickel-iron alloy-based catalyst for hydrogenating isophthalonitrile to meta-xylylenediamine according to claim 2, characterized in that: The sedimentation precipitation method comprises the following steps: S1: dissolving metal salts of Ni and Fe or metal salts of other transition metals Cu, Co, Sn in water to prepare a metal salt solution, adding a precipitant dropwise for precipitation, and adding a carrier to stir and mix evenly; S2. Drying and calcining the obtained precipitate to obtain the composite metal oxide catalyst.

6. A nickel-iron alloy-based catalyst for hydrogenating isophthalonitrile to meta-xylylenediamine according to any one of claims 3 to 5, characterized in that: The metal salt is one or more of nitrate, sulfate, halide and acetate; the precipitant is one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium hydroxide and potassium hydroxide.

7. Use of the nickel-iron alloy-based catalyst according to claim 1 in hydrogenating isophthalonitrile to produce meta-xylylenediamine.

8. The use according to claim 7, characterized in that: Isophthalonitrile is dissolved in liquid ammonia and a proper amount of organic solvent is added to prepare a raw material liquid, and in the presence of the nickel-iron alloy-based catalyst, the raw material liquid is reacted with hydrogen to obtain meta-xylylenediamine.

9. The use according to claim 7, characterized in that: The reaction conditions for preparing m-xylylenediamine by catalytic hydrogenation of isophthalonitrile are as follows: temperature 60-200° C., pressure 1-25 MPa, and isophthalonitrile space velocity 0.1-2.0 h -1 , the molar ratio of isophthalonitrile to hydrogen is 1:200, preferably 1:100.

Citation Information

Patent Citations

  • Catalyst for use in preparation of paraphenyldimethylamine and preparation method thereof

    CN102029160A

  • Catalyst for preparing m-xylylenediamine by isophthalonitrile hydrogenation under ammonia reaction conditions

    CN102688763A

  • Method for preparing m-xylylenediamine

    CN102690205A

  • Catalyst and method for preparing m-xylylenediamine by hydrogen isophthalonitrile

    CN104148080A

  • Preparation method of m-xylylenediamine

    CN107540556A