Coating method for improving adhesive force of paint

Through the treatment of chrome-plated brown corundum sand blasting and rust remover, the problem of insufficient adhesion of the paint film on the surface of the part is solved, the surface cleanliness and roughness is improved, the adhesion and durability of the paint film is enhanced, and the sand material is reduced. loss.

CN118950429APending Publication Date: 2024-11-15ZUNYI JINYE MASCH FOUNDRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411086167.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing painting process, the adhesion of the paint film on the surface of the part is insufficient, and the paint film is prone to fall off, affecting the decorative and protective properties.

Method used

The chrome-plated brown corundum sand is used for sandblasting treatment, and combined with rust remover atomization spraying and ultrasonic cleaning, improve surface cleanliness and roughness and enhance the adhesion of the paint film.

Benefits of technology

Effectively remove rust spots, improve the binding force between the part surface and the paint film, extend the durability of the paint film, reduce the loss of brown corundum sand, and enhance the adhesion and corrosion resistance of the paint film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985240290000091
    Figure BDA0004985240290000091
Patent Text Reader

Abstract

The invention discloses a coating method for improving the adhesive force of paint, and belongs to the technical field of paint. Surface treatment is conducted on a part before paint spraying by combining rust remover treatment and a sand blasting process, the standing reaction time of the rust remover sprayed on the surface of the part in an atomized mode is controlled, so that rust spots on the surface are loosened, the rust spots can be better removed through follow-up sand blasting treatment, chromium is plated on the surface of brown corundum sand, the toughness and corrosion resistance of sand materials can be improved, and the service life of the sand materials is prolonged. The sand blasting device is suitable for a sand blasting process after acid rust remover treatment, and the loss of sand is reduced. Through surface treatment of the part, the roughness is improved, rusty spots are reduced, the adhesive force of a paint film formed on the surface of the part through the paint spraying process is increased, the paint film is not prone to falling off, and the protection performance is better exerted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of paints, and in particular relates to a coating method for improving the adhesion of paints. Background Art

[0002] Painting is an important part of product manufacturing and is related to the appearance quality of the product. It not only gives the product excellent protection and decorative properties, but is also an important component of the product value. Parts painting is a common surface treatment process used to increase the aesthetics and corrosion resistance of parts. The adhesion of the paint film is one of the important indicators for assessing the performance of the paint film. Only when the paint film has a certain adhesion can it better adhere to the surface of the substrate, give full play to the decorative and protective properties of the paint, and achieve the purpose of applying the paint. In actual production, it was found that the paint film adhesion of arm parts after painting was insufficient, the cross-cut test failed, and even the paint film fell off in some parts. To solve this problem, the painting process needs to be improved.

[0003] The quality of pre-treatment affects the adhesion, appearance, moisture resistance and corrosion resistance of the coating. If the pre-treatment is not good, rust will continue to spread under the coating, causing the coating to fall off in pieces. Sandblasting has the advantages of high efficiency and high cleaning degree on the surface of parts compared with other methods.

[0004] Sandblasting uses compressed air as a power to form a high-speed jet beam, and sprays the material (copper ore sand, quartz sand, iron sand, sea sand, corundum, etc.) at high speed onto the surface of the part to be processed, so that the appearance of the outer surface of the part changes. Due to the impact and cutting action of the abrasive on the surface of the part, the surface of the part obtains a certain degree of cleanliness and different roughness, and the mechanical properties of the surface of the part are improved, thereby improving the fatigue resistance of the part, increasing the adhesion between it and the coating, and extending the durability of the coating. Brown corundum is an artificial crystal material made of bauxite by high-temperature smelting. Its crystal blocks are crushed and screened into brown corundum abrasives of different particle sizes for different grinding processing fields. In the actual sandblasting process, if the impact force of the sandblasting is not enough, the brown corundum will not be able to remove rust well, the bonding strength between the surface of the metal parts and the coating will decrease, and the coating will easily fall off. Summary of the invention

[0005] The purpose of the present invention is to provide a coating method for improving the adhesion of paint, so as to improve the adhesion of paint on the surface of parts.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] The present invention provides a coating method for improving the adhesion of paint, comprising the following steps:

[0008] S1. Assembly: Assemble the parts that have been machined and magnetic particle inspected;

[0009] S2. Protection before sandblasting: Use tooling to protect the parts that do not need to be painted;

[0010] S3, rust remover treatment: spray the rust remover on the surface of the parts by atomization and let it stand for reaction;

[0011] S3, sandblasting: Use chrome-plated brown corundum sand to sandblast the painted parts, and remove the sand and dust on the surface of the parts after sandblasting;

[0012] S4, ultrasonic cleaning: the sandblasted parts are cleaned in a three-step ultrasonic bubbling assisted cleaning tank, and then dried after cleaning;

[0013] S5. Assembly: Assemble according to the assembly process of each part;

[0014] S6. Scrub: Remove dust from the surface of parts, check the oil stains on the surface of parts and clean them, and wipe the surface dry with a dust-free cloth;

[0015] S7. Protection before painting: shield and protect the parts that do not need to be painted;

[0016] S8, painting: Use primer to spray paint the surface of parts once, dry it once, level it and remove dust, use topcoat to spray paint the surface of parts twice, and get the painted parts after the second drying.

[0017] Furthermore, the rust remover is at least one of hydrochloric acid solution, oxalic acid solution, citric acid solution and phosphoric acid solution; and the standing reaction time is 5-30 minutes.

[0018] Furthermore, the spray material is 60-mesh chrome-plated brown corundum sand, and the preparation method of the chrome-plated brown corundum sand is as follows:

[0019] Add the mineralizer into water and heat to dissolve, then add chromium nitrate into the solution while stirring to form a plating solution, mix the brown corundum sand and the plating solution for 10-20 minutes, the plating solution is 1%-5% of the mass of the brown corundum sand, dry it and treat it at 500-600℃ for 3h, and cool it to obtain the chrome-plated brown corundum sand.

[0020] Furthermore, during the sandblasting process, ultrasonic vibration of the parts assists the sandblasting.

[0021] Furthermore, the air pressure of the sandblasting treatment is 0.7 MPa, and the nozzle is 100-300 mm away from the surface of the part.

[0022] Furthermore, the tank liquid in the cleaning tank is a mixture of a cleaning agent and water or a mixture of a rinsing agent and water;

[0023] The cleaning agent is KA-T110; the rinsing agent is KA-F150.

[0024] Furthermore, the three-step ultrasonic bubbling assisted cleaning includes:

[0025] (1) Step 1: Place parts in a cleaning tank, heat the 6 wt% cleaning agent solution to 60-70°C, and perform ultrasonic and bubbling assisted cleaning for 15 minutes;

[0026] (2) Step 2: Place the parts after the first step into a 5 wt% cleaning agent bath and keep the temperature at 60-70°C, and perform ultrasonic and bubbling assisted cleaning for 15 minutes;

[0027] (3) Step 3: Place the parts after step 2 into a 5 wt% rinse agent bath at 40°C and perform bubbling cleaning for 15 minutes.

[0028] The three-step ultrasonic cleaning can fully remove dust and oil on the surface of parts, improve the cleanliness of the surface, and make the surface of parts and paint evenly and flawlessly combined.

[0029] Furthermore, the nozzle of the first spray painting treatment is 20-30 cm away from the surface of the part, and the air pressure of the spray gun is 0.2-0.5 MPa.

[0030] Furthermore, the drying temperature of the primary drying is 80° C., and the primary drying time is 2-3 hours.

[0031] Furthermore, the secondary drying temperature is 50-60° C., and the secondary drying time is 2 hours.

[0032] Beneficial effects of the present invention:

[0033] (1) The present invention adds rust remover treatment and sandblasting process before painting, and the rust remover is atomized and sprayed on the surface of the parts. During the static process, the rust remover and the rust spots on the surface react. The atomized spraying avoids excessive corrosion of the surface by the rust remover. After the reaction, the rust spots on the surface are loosened. Combined with the spraying of the sandblasting process, the rust spots on the surface and the excess acid can be removed, and the surface roughness of the parts can be improved, so that the surface primer has greater adhesion, which is beneficial to prevent the paint film from falling off.

[0034] (2) The present invention uses chrome-plated brown corundum sand as the blasting material, which can improve the corrosion resistance and compressive strength of the brown corundum sand, increase the impact force on the surface of the parts during the sandblasting process, and reduce the loss of brown corundum sand. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] Preparation of chrome-plated brown corundum sand:

[0038] Add the mineralizer into water and heat to dissolve, then add chromium nitrate into the solution while stirring to form a plating solution, mix the brown corundum sand and the plating solution for 20 minutes, the plating solution is 1% of the mass of the brown corundum sand, dry it, treat it at 500℃ for 3 hours, and cool it to obtain the chrome-plated brown corundum sand.

[0039] Parts surface coating:

[0040] S1. Assembly: Assemble the parts that have been machined and magnetic particle inspected;

[0041] S2. Protection before sandblasting: Use tooling to protect the parts that do not need to be painted;

[0042] S3, rust remover treatment: spray a 5wt% hydrochloric acid solution on the surface of the part by atomization, and let it react for 10 minutes;

[0043] S3, sandblasting: Use 60 mesh chrome-plated brown corundum sand to sandblast the painted parts. The air pressure for sandblasting is 0.7MPa, and the nozzle is 300mm away from the surface of the part. During the sandblasting process, the parts are assisted by ultrasonic vibration. After the sandblasting is completed, the sand and dust on the surface of the parts are removed;

[0044] S4, ultrasonic cleaning: the parts after sandblasting are subjected to three-step ultrasonic bubbling assisted cleaning in the cleaning tank, and then dried after cleaning. The three-step ultrasonic bubbling assisted cleaning includes:

[0045] (1) Step 1: Put the parts into the cleaning tank, heat the tank liquid containing 6wt% KA-T110 cleaning agent to 70°C, and clean them for 15 minutes with ultrasound and bubbling assistance;

[0046] (2) Step 2: Place the parts after the first step into a bath containing 5 wt% KA-T110 cleaning agent and keep it at 60°C, and clean them with ultrasound and bubbling for 15 minutes;

[0047] (3) Step 3: Place the parts after step 2 into a bath containing 5 wt% KA-F150 rinse agent at 40°C and perform bubbling cleaning for 15 minutes.

[0048] S5. Assembly: Assemble according to the assembly process of each part.

[0049] S6. Scrub: Remove dust from the surface of parts, check the oil stains on the surface of parts and clean them, and wipe the surface dry with a dust-free cloth;

[0050] S7. Protection before painting: shield and protect the parts that do not need to be painted;

[0051] S8. Painting: Use primer to spray paint the surface of the parts once, the nozzle is 25cm away from the part surface, the air pressure of the spray gun is 0.3MPa, and the parts are leveled and dusted after one drying. The drying temperature is set to 80℃ and the drying time is 2h. Use topcoat to spray paint the surface of the parts for the second time. After the second drying, the painted parts are obtained. The drying temperature is set to 60℃ and the drying time is 2h.

[0052] Example 2

[0053] The difference from Example 1 is that the plating solution is adjusted from 1% of the mass of the brown corundum sand to 3%, and the other steps are the same as Example 1.

[0054] Example 3

[0055] The difference from Example 1 is that the plating solution is adjusted from 1% of the mass of the brown corundum sand to 5%, and the other steps are the same as Example 1.

[0056] Example 4

[0057] The difference from Example 1 is that the standing time in the rust remover treatment is adjusted to 5 minutes, and the other steps are the same as Example 1.

[0058] Example 5

[0059] The difference from Example 1 is that the standing time in the rust remover treatment is adjusted to 15 minutes, and the other steps are the same as Example 1.

[0060] Example 6

[0061] Preparation of chrome-plated brown corundum sand:

[0062] Add the mineralizer into water and heat to dissolve, then add chromium nitrate into the solution while stirring to form a plating solution, mix the brown corundum sand and the plating solution for 10 minutes, the plating solution is 1% of the mass of the brown corundum sand, dry it, treat it at 550℃ for 3 hours, and cool it to obtain the chrome-plated brown corundum sand.

[0063] Parts surface coating:

[0064] S1. Assembly: Assemble the parts that have been machined and magnetic particle inspected;

[0065] S2. Protection before sandblasting: Use tooling to protect the parts that do not need to be painted;

[0066] S3, rust remover treatment: spray a 10wt% phosphoric acid solution on the surface of the part by atomization, and let it react for 30 minutes;

[0067] S3, sandblasting: Use 60 mesh chrome-plated brown corundum sand to sandblast the painted parts. The air pressure for sandblasting is 0.7MPa, and the nozzle is 200mm away from the surface of the part. During the sandblasting process, the parts are assisted by ultrasonic vibration. After the sandblasting is completed, the sand and dust on the surface of the parts are removed;

[0068] S4, ultrasonic cleaning: the parts after sandblasting are subjected to three-step ultrasonic bubbling assisted cleaning in the cleaning tank, and then dried after cleaning. The three-step ultrasonic bubbling assisted cleaning includes:

[0069] (1) Step 1: Put the parts into the cleaning tank, heat the tank liquid containing 6wt% KA-T110 cleaning agent to 65°C, and clean them with ultrasound and bubbling for 15 minutes;

[0070] (2) Step 2: Place the parts after the first step into a bath containing 5 wt% KA-T110 cleaning agent and keep the temperature at 70°C, and perform ultrasonic and bubbling assisted cleaning for 15 minutes;

[0071] (3) Step 3: Place the parts after step 2 into a bath containing 5 wt% KA-F150 rinse agent at 40°C and perform bubbling cleaning for 15 minutes.

[0072] S5. Assembly: Assemble according to the assembly process of each part.

[0073] S6. Scrub: Remove dust from the surface of parts, check the oil stains on the surface of parts and clean them, and wipe the surface dry with a dust-free cloth;

[0074] S7. Protection before painting: shield and protect the parts that do not need to be painted;

[0075] S8. Painting: Use primer to spray paint the surface of the parts once, the nozzle is 20cm away from the surface of the parts, the air pressure of the spray gun is 0.2MPa, and the parts are leveled and dusted after one drying. The drying temperature is set to 80℃ and the drying time is 2.5h. Use topcoat to spray paint the surface of the parts for the second time. After the second drying, the painted parts are obtained. The drying temperature is set to 55℃ and the drying time is 2h.

[0076] Example 7

[0077] Preparation of chrome-plated brown corundum sand:

[0078] Add the mineralizer into water and heat to dissolve, then add chromium nitrate into the solution while stirring to form a plating solution, mix the brown corundum sand and the plating solution for 15 minutes, the plating solution is 1% of the mass of the brown corundum sand, dry it and treat it at 600℃ for 3 hours, and cool it to obtain the chrome-plated brown corundum sand.

[0079] Parts surface coating:

[0080] S1. Assembly: Assemble the parts that have been machined and magnetic particle inspected;

[0081] S2. Protection before sandblasting: Use tooling to protect the parts that do not need to be painted;

[0082] S3, rust remover treatment: spray 10wt% oxalic acid solution on the surface of the parts by atomization, and let it react for 20 minutes;

[0083] S3, sandblasting: Use 60 mesh chrome-plated brown corundum sand to sandblast the painted parts. The air pressure for sandblasting is 0.7MPa, and the nozzle is 100mm away from the surface of the part. During the sandblasting process, the parts are assisted by ultrasonic vibration. After the sandblasting is completed, the sand and dust on the surface of the parts are removed;

[0084] S4, ultrasonic cleaning: the parts after sandblasting are subjected to three-step ultrasonic bubbling assisted cleaning in the cleaning tank, and then dried after cleaning. The three-step ultrasonic bubbling assisted cleaning includes:

[0085] (1) Step 1: Put the parts into the cleaning tank, heat the tank liquid containing 6wt% KA-T110 cleaning agent to 60°C, and clean them with ultrasound and bubbling for 15 minutes;

[0086] (2) Step 2: Place the parts after the first step into a bath containing 5 wt% KA-T110 cleaning agent and keep the temperature at 65°C, and perform ultrasonic and bubbling assisted cleaning for 15 minutes;

[0087] (3) Step 3: Place the parts after step 2 into a bath containing 5 wt% KA-F150 rinse agent at 40°C and perform bubbling cleaning for 15 minutes.

[0088] S5. Assembly: Assemble according to the assembly process of each part.

[0089] S6. Scrub: Remove dust from the surface of parts, check the oil stains on the surface of parts and clean them, and wipe the surface dry with a dust-free cloth;

[0090] S7. Protection before painting: shield and protect the parts that do not need to be painted;

[0091] S8. Painting: Use primer to spray paint the surface of the parts once, with the nozzle 30cm away from the surface of the parts and the air pressure of the spray gun at 0.5MPa. After one drying, level and remove dust. Set the drying temperature to 80℃ and the drying time to 3h. Use topcoat to spray paint the surface of the parts for the second time. After the second drying, the painted parts are obtained. Set the drying temperature to 50℃ and the drying time to 2h.

[0092] Comparative Example 1

[0093] Compared with Example 1, the difference is that no rust remover treatment is performed before sandblasting, and the other steps are the same as Example 1.

[0094] Comparative Example 2

[0095] Compared with Example 1, the difference is that no sandblasting is performed, and the other steps are the same as Example 1.

[0096] Comparative Example 3

[0097] Compared with Example 1, the difference is that no rust remover treatment and sandblasting are performed, and the other steps are the same as Example 1.

[0098] Comparative Example 4

[0099] Compared with Example 1, the difference is that 60-mesh brown corundum sand is used for sandblasting, and the other steps are the same as Example 1.

[0100] Performance tests were performed on Examples 1 to 7 and Comparative Examples 1 to 4, and the results are shown in Table 1.

[0101] The paint film adhesion test refers to "GB / T 9286-2021 Scratch test for paints and varnishes".

[0102] Blast cleaning level: Refer to GB / T 8923.1-2011 Surface preparation of steel before coating - Visual assessment of surface cleanliness - Part 1: Rust grades and treatment grades for uncoated steel surfaces and steel surfaces after complete removal of the original coating for parts after sandblasting.

[0103] The loss of chrome-plated brown corundum sand is calculated according to the mass ratio of the unbroken sand after sandblasting to the sand before sandblasting.

[0104] The surface roughness test of parts after sandblasting refers to "GB / T 13288.1-2008 Surface preparation of steel before coating - Surface roughness characteristics of steel after blast cleaning - Part 1: Technical requirements and definitions of ISO surface roughness comparison specimens for evaluating the surface roughness of steel after blast cleaning".

[0105] Table 1

[0106]

[0107] As can be seen from Table 1, adding rust remover treatment is beneficial to removing surface rust spots. It can improve the adhesion of the paint film, and the rust remover is left on the surface for too short a reaction time, the rust removal is incomplete, and the time is too long, which may cause corrosion to the parts material. Adding sandblasting before painting is beneficial to removing surface dirt, improving surface roughness, and improving the adhesion of the paint film. Chrome plating the surface of brown corundum sand can increase the toughness of the sand material. There is acid on the surface of the parts treated with rust remover, which will corrode the sand material. Chrome plating can improve corrosion resistance and reduce loss. The mass proportion of the plating solution is increased, which greatly reduces the loss.

[0108] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0109] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A coating method for improving paint adhesion, characterized in that: The steps include: S1. Assembly: Assemble the parts that have been machined and magnetic particle inspected; S2. Protection before sandblasting: Use tooling to protect the parts that do not need to be painted; S3, rust remover treatment: spray the rust remover on the surface of the parts by atomization and let it stand for reaction; S3, sandblasting: Use chrome-plated brown corundum sand to sandblast the painted parts, and remove the sand and dust on the surface of the parts after sandblasting; S4, ultrasonic cleaning: the sandblasted parts are cleaned in a three-step ultrasonic bubbling assisted cleaning tank, and then dried after cleaning; S5. Assembly: Assemble according to the assembly process of each part; S6. Scrub: Remove dust from the surface of parts, check the oil stains on the surface of parts and clean them, and wipe the surface dry with a dust-free cloth; S7. Protection before painting: shield and protect the parts that do not need to be painted; S8, painting: Use primer to spray paint the surface of parts once, dry it once, level it and remove dust, use topcoat to spray paint the surface of parts twice, and get the painted parts after the second drying.

2. A coating method for improving paint adhesion according to claim 1, characterized in that: The rust remover is at least one of hydrochloric acid solution, oxalic acid solution, citric acid solution and phosphoric acid solution; and the standing reaction time is 5-30 minutes.

3. A coating method for improving paint adhesion according to claim 1, characterized in that: The spray material is 60-mesh chrome-plated brown corundum sand, and the preparation method of the chrome-plated brown corundum sand is as follows: Add the mineralizer into water and heat to dissolve, then add chromium nitrate into the solution while stirring to form a plating solution, mix the brown corundum sand and the plating solution for 10-20 minutes, the plating solution is 1%-5% of the mass of the brown corundum sand, dry it and treat it at 500-600℃ for 3h, and cool it to obtain the chrome-plated brown corundum sand.

4. A coating method for improving paint adhesion according to claim 1, characterized in that: In the sandblasting process, ultrasonic vibration of the parts assists the sandblasting.

5. A coating method for improving paint adhesion according to claim 1, characterized in that: The air pressure of the sandblasting treatment is 0.7 MPa, and the nozzle is 100-300 mm away from the surface of the part.

6. A coating method for improving paint adhesion according to claim 1, characterized in that: The tank liquid in the cleaning tank is a mixture of a cleaning agent and water or a mixture of a rinsing agent and water; The cleaning agent is KA-T110; the rinsing agent is KA-F150.

7. A coating method for improving paint adhesion according to claim 1, characterized in that: The three-step ultrasonic bubbling assisted cleaning includes: (1) Step 1: Place parts in a cleaning tank, heat the 6 wt% cleaning agent solution to 60-70°C, and perform ultrasonic and bubbling assisted cleaning for 15 minutes; (2) Step 2: Place the parts after the first step into a 5 wt% cleaning agent bath and keep the temperature at 60-70°C, and perform ultrasonic and bubbling assisted cleaning for 15 minutes; (3) Step 3: Place the parts after step 2 into a 5 wt% rinse agent bath at 40°C and perform bubbling cleaning for 15 minutes.

8. A coating method for improving paint adhesion according to claim 1, characterized in that: The nozzle of the first spray painting process is 20-30 cm away from the surface of the part, and the air pressure of the spray gun is 0.2-0.5 MPa.

9. A coating method for improving paint adhesion according to claim 1, characterized in that: The drying temperature of the primary drying is 80° C., and the primary drying time is 2-3 hours.

10. A coating method for improving paint adhesion according to claim 1, characterized in that: The secondary drying temperature is 50-60° C., and the secondary drying time is 2 hours.