Preparation method of colored glaze powder artwork formed by binder injection
The glass powder is printed through adhesive spray molding technology, combined with drying and degreasing sintering treatment, which solves the problem of low success rate of glass products, and achieves efficient and exquisite art production, reducing costs and improving success rate.
Patent Information
- Application Number
- CN202411050196.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
The fire success rate of existing glazed products is low, resulting in burnt parts being invalidated, and the traditional handmade blank making process is cumbersome, which limits the design and production efficiency of the artwork.
Adhesive spray molding technology, glass powder is mixed with a specific ratio of adhesive, printed and molded through an adhesive jet printer, and then dried, degreased and sintered and polished to form a work of art.
It improves the success rate of glass products, reduces manual operations, achieves more efficient production, can reorganize and utilize burned parts, reduce costs, breaks through structural limitations, and improves the quality and automation of artworks.
Smart Images

Figure CN118952884A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of binder injection molding, and more particularly to a method for preparing a binder injection molded glass powder artwork. Background Art
[0002] As an art piece with a long history, colored glaze products have always been made by making mold frames, then hand-made blanks, and then fired. However, the firing success rate is generally only 40%-60%, and the burned colored glaze pieces can only be scrapped.
[0003] Therefore, how to improve the success rate of glass products is a problem that those skilled in the art need to solve urgently. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a method for preparing a glass powder artwork formed by adhesive injection molding to solve the deficiencies in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for preparing a glass powder artwork formed by adhesive injection molding, specifically comprising the following steps:
[0007] (1) crushing glass into powder, adding sodium hydroxymethyl cellulose, mixing evenly, spheroidizing, and sieving to obtain glass powder;
[0008] (2) mixing with purified water and heating; stirring the purified water and uniformly mixing with sodium hydroxymethyl cellulose; mixing with glacial acetic acid and mixing and stirring; cooling, mixing with ethylene glycol and mixing and stirring; mixing with sorbitol and mixing and stirring; mixing with ethylene glycol butyl ether and mixing and stirring to obtain a binder;
[0009] (3) placing glass powder and binder into corresponding positions of a binder jet printer, slicing according to the required model, and importing the slice file into the device for printing to obtain a green body;
[0010] (4) placing the green body into an oven for drying and solidification to obtain a colored glaze piece;
[0011] (5) taking out the colored glaze piece, cleaning the floating powder; putting it into a degreasing sintering furnace, degreasing and sintering; grinding and polishing to obtain a green body;
[0012] (6) The body is glazed, painted, and baked for the second time to obtain a binder-injected glass powder artwork.
[0013] Furthermore, in the above step (1), the particles are crushed to a particle size of 100-300 mesh.
[0014] Furthermore, in the above step (1), the amount of sodium hydroxymethyl cellulose added is 10% of the mass of the glass powder.
[0015] A further beneficial effect of the above method is that sodium hydroxymethyl cellulose as a dispersant can increase the fluidity of the glass powder, increase the bonding degree of the binder, and increase the strength of the green body.
[0016] Furthermore, in the above step (2), the weight proportions of the raw materials in the binder are: 100-200 parts of purified water, 40-50 parts of sodium hydroxymethyl cellulose, 5-10 parts of glacial acetic acid, 5-8 parts of ethylene glycol, 2-5 parts of sorbitol, and 1-2 parts of ethylene glycol butyl ether.
[0017] Furthermore, the weight proportions of the raw materials in the above-mentioned binder are: 100 parts of purified water, 40 parts of sodium hydroxymethyl cellulose, 5 parts of glacial acetic acid, 5 parts of ethylene glycol, 2 parts of sorbitol, and 1 part of ethylene glycol butyl ether.
[0018] Furthermore, the weight proportions of the raw materials in the above-mentioned binder are: 200 parts of purified water, 50 parts of sodium hydroxymethyl cellulose, 10 parts of glacial acetic acid, 8 parts of ethylene glycol, 5 parts of sorbitol, and 2 parts of ethylene glycol butyl ether.
[0019] The further beneficial effect of adopting the above is that pure water is used as a solvent to dissolve the raw materials; sodium hydroxymethyl cellulose is used as the main body of the binder to play an adhesive role; glacial acetic acid acts as a catalyst to accelerate the mixed dissolution of the raw materials and acts as a volatile solvent to quickly solidify during printing; ethylene glycol and ethylene glycol butyl ether are used as surfactants to adjust the viscosity of the binder; sorbitol is used as a stabilizer to stabilize the binder and prevent it from deteriorating.
[0020] Furthermore, in the above step (2), the mixture is heated to 85°C; the stirring speed of the pure water is 100 r / min; the stirring time for mixing in glacial acetic acid is 30 min; the mixture is cooled to room temperature; the stirring time for mixing in ethylene glycol is 10 min; the stirring time for mixing in sorbitol is 10 min; and the stirring time for mixing in ethylene glycol butyl ether is 10 min.
[0021] Furthermore, in the above step (4), the drying and curing temperature is 200° C. and the time is 3 hours.
[0022] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0023] 1. The preparation method of the present invention includes processes such as glass powder processing, binder preparation, curing treatment, powder cleaning, degreasing sintering and polishing. The glass powder used first can be new glass powder mixed and prepared by spheroidization treatment, or it can be powdered glass pieces that failed to be fired; then put it into the binder jet printer, and use the prepared binder for inkjet bonding molding; then it is cured and strengthened, and the powder is cleaned; then it is degreased and sintered, and then the surface is polished and polished to increase the surface gloss to become an art piece blank. After the blank is completed, it can replace the traditional handmade glass blank.
[0024] 2. The present invention combines the new technology of binder injection with the traditional process technology. On the one hand, it reduces labor, and the resulting blank is more refined and has a higher success rate. On the other hand, the burned glass pieces can be broken and reassembled and re-molded, saving a lot of costs. This is a breakthrough in the development of glass artworks.
[0025] 3. The preparation method of the present invention can break through the art products of arbitrary structures that cannot be completed by hand, ignoring the structural limitations; reducing labor, no need for years of experience in handicrafts, fast mold forming speed, shortening the production cycle; high degree of automation, improved yield; failed firing products can be recycled and reused, saving a lot of materials.
[0026] 4. The present invention can be used for the shaping of colored glaze artworks, thereby improving the quality of colored glaze artworks and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a physical picture of the green body prepared in Example 1. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] The preparation method of the binder spray-molded glass powder artwork specifically comprises the following steps:
[0031] (1) crushing glass into powder with a particle size of 100-300 mesh, adding 10% by weight of sodium hydroxymethyl cellulose, mixing evenly, spheroidizing, and sieving to obtain glass powder;
[0032] (2) adding 100 g of purified water and heating to 85° C.; stirring the purified water at a speed of 100 r / min, uniformly adding 40 g of sodium hydroxymethyl cellulose; adding 5 g of glacial acetic acid and mixing and stirring for 30 min; cooling to room temperature, adding 5 g of ethylene glycol and mixing and stirring for 10 min; adding 2 g of sorbitol and mixing and stirring for 10 min; adding 1 g of ethylene glycol butyl ether and mixing and stirring for 10 min to obtain a binder;
[0033] (3) Place the glass powder and binder in the corresponding position of the binder jet printer, slice according to the required model, import the slice file into the device, print the glass three-dimensional model, and obtain the green body (such as Figure 1 shown);
[0034] (4) placing the green body into an oven and drying and curing at 200° C. for 3 h to obtain a glass piece;
[0035] (5) taking out the colored glaze piece, cleaning the floating powder; putting it into a degreasing sintering furnace, degreasing and sintering; grinding and polishing to obtain a green body;
[0036] (6) The body is glazed, painted, and baked for the second time to obtain a binder-injected glass powder artwork.
[0037] Example 2
[0038] The preparation method of the binder spray-molded glass powder artwork specifically comprises the following steps:
[0039] (1) crushing glass into powder with a particle size of 100-300 mesh, adding 10% by weight of sodium hydroxymethyl cellulose, mixing evenly, spheroidizing, and sieving to obtain glass powder;
[0040] (2) adding 200 g of purified water and heating to 85° C.; stirring the purified water at a speed of 100 r / min, uniformly adding 50 g of sodium hydroxymethyl cellulose; adding 10 g of glacial acetic acid and mixing and stirring for 30 min; cooling to room temperature, adding 8 g of ethylene glycol and mixing and stirring for 10 min; adding 5 g of sorbitol and mixing and stirring for 10 min; adding 2 g of ethylene glycol butyl ether and mixing and stirring for 10 min to obtain a binder;
[0041] (3) placing glass powder and binder into corresponding positions of the binder jet printer, slicing according to the required model, and importing the slice file into the device to print the glass three-dimensional model to obtain a green body;
[0042] (4) placing the green body into an oven and drying and curing at 200° C. for 3 h to obtain a glass piece;
[0043] (5) taking out the colored glaze piece, cleaning the floating powder; putting it into a degreasing sintering furnace, degreasing and sintering; grinding and polishing to obtain a green body;
[0044] (6) The body is glazed, painted, and baked for the second time to obtain a binder-injected glass powder artwork.
[0045] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a glass powder artwork by binder injection molding, characterized in that: The specific steps include: (1) crushing glass into powder, adding sodium hydroxymethyl cellulose, mixing evenly, spheroidizing, and sieving to obtain glass powder; (2) Add purified water and heat; stir the purified water and evenly mix in sodium hydroxymethyl cellulose; add glacial acetic acid and mix and stir; Cooling, mixing into ethylene glycol, mixing and stirring; mixing into sorbitol, mixing and stirring; mixing into ethylene glycol butyl ether, mixing and stirring to obtain a binder; (3) Place the glass powder and binder in the corresponding position of the binder jet printer, slice according to the required model, import the slice file into the device, print and shape, and obtain the green body; (4) placing the green body into an oven for drying and solidification to obtain a colored glaze piece; (5) Take out the glass piece, clean the loose powder; put it into the degreasing sintering furnace, degreasing and sintering; grind and polish to obtain the green body; (6) The body is glazed, painted, and baked twice to obtain the binder-injected glass powder artwork.
2. The method for preparing a binder-injection-molded glass powder artwork according to claim 1, characterized in that: In step (1), the crushing is performed to a particle size of 100-300 meshes.
3. The method for preparing a binder-injection-molded glass powder artwork according to claim 1, characterized in that: In step (1), the amount of sodium hydroxymethyl cellulose added is 10% of the mass of the glass powder.
4. The method for preparing a binder-injection-molded glass powder artwork according to claim 1, characterized in that: In step (2), the weight proportions of the raw materials in the binder are: 100-200 parts of purified water, 40-50 parts of sodium hydroxymethyl cellulose, 5-10 parts of glacial acetic acid, 5-8 parts of ethylene glycol, 2-5 parts of sorbitol, and 1-2 parts of ethylene glycol butyl ether.
5. The method for preparing a binder-injection-molded glass powder artwork according to claim 4, characterized in that: The weight proportions of the raw materials in the binder are: 100 parts of purified water, 40 parts of sodium hydroxymethyl cellulose, 5 parts of glacial acetic acid, 5 parts of ethylene glycol, 2 parts of sorbitol, and 1 part of ethylene glycol butyl ether.
6. The method for preparing a binder-injection-molded glass powder artwork according to claim 4, characterized in that: The weight proportions of the raw materials in the binder are as follows: 200 parts of purified water, 50 parts of sodium hydroxymethyl cellulose, 10 parts of glacial acetic acid, 8 parts of ethylene glycol, 5 parts of sorbitol, and 2 parts of ethylene glycol butyl ether.
7. The method for preparing a binder-injection-molded glass powder artwork according to claim 1, characterized in that: In step (2), the heating is to 85° C.; the pure water is stirred at a speed of 100 r / min; the stirring time for mixing in glacial acetic acid is 30 min; the cooling is to room temperature; the stirring time for mixing in ethylene glycol is 10 min; the stirring time for mixing in sorbitol is 10 min; and the stirring time for mixing in ethylene glycol butyl ether is 10 min.
8. The method for preparing a glass powder artwork formed by binder injection molding according to claim 1, characterized in that: In step (4), the drying and curing temperature is 200° C. and the time is 3 hours.