Lightweight double-oriented high-thermal-conductivity graphene foam material and preparation method thereof
By introducing high thermal conductivity carbon fibers into graphene foam and adopting sandwich structural design, the existing high thermal conductivity materials have been solved, and the graphene foam materials with lightweight, high thermal conductivity and excellent mechanical properties have been achieved. Suitable for low energy consumption fields.
Patent Information
- Application Number
- CN202410885206.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-15
AI Technical Summary
The application of existing high thermal conductivity materials in some fields is limited by their high density and processing difficulty. At the same time, the thermal conductivity of non-metallic materials such as graphene is mainly concentrated in one direction and is difficult to effectively apply in the field of low energy consumption.
Lightweight double-oriented high thermal graphene foam material with a sandwich structure composed of horizontally oriented graphene foam/vertical oriented graphene foam/horizontal oriented graphene foam, combined with high thermal carbon fiber to improve mechanical properties, and through simple, safe and environmental protection The preparation method reduces the overall density.
It realizes the low density, high in-plane and inter-plane thermal conductivity of the material, excellent mechanical properties, can be continuously compressed 10,000 times without basically changing the morphology, and is suitable for low energy consumption fields.
Smart Images

Figure CN118954490A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of materials, and in particular to a lightweight dual-oriented high thermal conductivity graphene foam material and a preparation method thereof. Background Art
[0002] With the rapid development of modern science and technology, the integration and power density of electronic devices are constantly increasing, resulting in thermal management issues becoming an important factor affecting their performance and reliability. High thermal conductivity materials, due to their excellent thermal conductivity, can effectively transfer heat from heat sources to heat dissipation components, thereby improving the working efficiency and life of electronic devices. In addition, high thermal conductivity materials also have broad application prospects in energy management, aerospace, automotive industry and other fields, such as heat recovery, engine cooling and thermal protection of structural parts.
[0003] At present, the research on high thermal conductivity materials is mainly focused on three categories: metal materials, non-metallic materials and composite materials. Metal materials such as copper and aluminum are widely used due to their excellent thermal conductivity, but their high density and processing difficulty limit their application in certain fields. Non-metallic materials such as carbon-based materials have the advantages of high thermal conductivity and low density. For example, the thermal conductivity of graphene is as high as 3000-5000W / m·K, which is far higher than traditional materials such as copper and aluminum. However, due to its lamellar elementary structure, the thermal conductive materials prepared at present usually have high thermal conductivity only in one direction, and their high thermal conductivity is usually proportional to the density, which is not conducive to the application of materials in fields such as aerospace that urgently need low energy consumption. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a lightweight dual-oriented high thermal conductivity graphene foam material and a preparation method thereof. The material consists of a sandwich structure of horizontally oriented graphene foam / vertically oriented graphene foam / horizontally oriented graphene foam, wherein the horizontally oriented graphene foam has a higher density and provides a high in-plane thermal conductivity, and the vertically oriented graphene foam has a lower density, which effectively reduces the density of the overall material while providing a high inter-plane thermal conductivity; high thermal conductivity carbon fibers are introduced into the graphene foam, and the fiber structure is interlaced inside the foam to connect graphene sheets, thereby effectively improving the mechanical properties of the material; and the material preparation method is simple, safe and environmentally friendly, and has great application prospects.
[0005] In a first aspect of the present invention, the present invention provides a graphene foam material. According to an embodiment of the present invention, the material comprises: a bottom layer, an intermediate layer and a surface layer,
[0006] The bottom layer is horizontally oriented graphene foam;
[0007] The middle layer is vertically oriented graphene foam;
[0008] The surface layer is horizontally oriented graphene foam;
[0009] The density of the horizontally oriented graphene foam is higher than the density of the vertically oriented graphene foam;
[0010] The bottom layer, the middle layer and the surface layer all contain high thermal conductivity carbon fibers;
[0011] The density of the material is 30-70 mg cm -3 .
[0012] The material according to the embodiment of the present invention is composed of a sandwich structure of horizontally oriented graphene foam / vertically oriented graphene foam / horizontally oriented graphene foam, wherein the horizontally oriented graphene foam has a higher density and provides a high in-plane thermal conductivity, and the vertically oriented graphene foam has a lower density, which effectively reduces the density of the overall material while providing a high inter-plane thermal conductivity; high thermal conductivity carbon fibers are introduced into the graphene foam, and the fiber structure is interlaced inside the foam to connect the graphene sheets, effectively improving the mechanical properties of the material. The material according to the embodiment of the present invention has a low density, light weight, and excellent mechanical properties. It can be continuously compressed 10,000 times without substantially changing its morphology, and at the same time has ultra-high in-plane and inter-plane thermal conductivity, and is currently a very high thermal conductivity among foam-type lightweight materials.
[0013] According to an embodiment of the present invention, the above material may further include at least one of the following additional technical features:
[0014] According to an embodiment of the present invention, the thickness ratio of the horizontally oriented graphene foam to the vertically oriented graphene foam is 1:7-1:10. According to an embodiment of the present invention, this thickness ratio is a better ratio combining light weight and high thermal conductivity. Below this ratio, the proportion of the middle low-density part is too high, the foam is light but the thermal conductivity is reduced; above this ratio, the proportion of the upper and lower horizontally oriented high-density parts is too high, the material has good thermal conductivity, but the density is too high.
[0015] According to an embodiment of the present invention, the density of the horizontally oriented graphene foam is 80-170 mg cm -3 According to an embodiment of the present invention, this density range is a relatively optimal ratio that combines light weight and high thermal conductivity. If the density is too high, the material as a whole is too heavy; if the density is too low, the thermal conductivity of the material is reduced.
[0016] According to an embodiment of the present invention, the pore size of the horizontally oriented graphene foam is 5-50 μm. According to an embodiment of the present invention, this pore size range is a better ratio of light weight and high thermal conductivity. If the pore size is too small, the material is too heavy; if the density is too large, the thermal conductivity of the material is reduced.
[0017] According to an embodiment of the present invention, the density of the vertically oriented graphene foam is 30-60 mg cm -3According to an embodiment of the present invention, this density range is a relatively optimal ratio combining light weight and high thermal conductivity. If the density is too high, the material as a whole is too heavy; if the density is too low, the thermal conductivity of the material is reduced.
[0018] According to an embodiment of the present invention, the pore size of the vertically oriented graphene foam is 30-110 μm. According to an embodiment of the present invention, this pore size range is a better ratio of light weight and high thermal conductivity. If the pore size is too small, the material is too heavy; if the density is too large, the thermal conductivity of the material is reduced.
[0019] According to an embodiment of the present invention, the diameter of the high thermal conductivity carbon fiber is 20-50 μm. According to an embodiment of the present invention, the diameter of the high thermal conductivity carbon fiber will affect its thermal conductivity and dispersibility. In this diameter range, the carbon fiber exhibits excellent thermal conductivity and dispersibility at the same time. For carbon fiber, the smaller the size, the better the dispersibility, but as the diameter decreases, its thermal conductivity will also decrease rapidly. Therefore, below this value, the thermal conductivity of the final material decreases; above this value, the dispersion of the carbon fiber is affected, and the internal structure of the final material is uneven, affecting its overall thermal conductivity, mechanical properties, etc.
[0020] According to an embodiment of the present invention, the length of the high thermal conductivity carbon fiber is 200-1000 μm. According to an embodiment of the present invention, the length of the high thermal conductivity carbon fiber affects its dispersibility in graphene oxide and the thermal conductivity and mechanical properties of the final graphene foam. This length can achieve optimal overall performance. Below this length, it is difficult for carbon fiber to effectively intersperse between graphene layers and form bridges, so the thermal conductivity and mechanical properties of the material deteriorate. Above this length, the dispersibility of carbon fiber and graphene oxide is limited, and it is difficult to form a uniform orientation structure, which affects the integrity and mechanical properties of the final material.
[0021] According to an embodiment of the present invention, the graphene exists in the form of graphene oxide.
[0022] According to an embodiment of the present invention, the mass ratio of graphene oxide to carbon fiber is 1:5-1:30. According to an embodiment of the present invention, this mass ratio enables the composite material to have complete formability, excellent mechanical properties and thermal conductivity at the same time. Graphite oxide dispersion is prone to cracking during the rapid freezing process of liquid nitrogen. In the initial stage of preparation, carbon fiber and GO are evenly mixed, and carbon fiber can be interspersed between graphene oxide sheets, effectively inhibiting the generation of cracks. If it is higher than this ratio, that is, the amount of carbon fiber is too little, it is difficult to effectively inhibit the generation of cracks during the preparation freezing process; if it is lower than this ratio, that is, the carbon fiber content is too much, the GO solution will be too viscous, the contact between the GO sheets will be reduced, and the integrity and mechanical properties of the material after carbonization will deteriorate.
[0023] In another aspect of the present invention, the present invention also provides a method for preparing a graphene foam material. According to an embodiment of the present invention, the method comprises:
[0024] (1) mixing a graphene oxide dispersion and a high thermal conductivity carbon fiber to obtain a mixed graphene oxide dispersion;
[0025] (2) freezing and drying the mixed graphene oxide dispersion to obtain vertically oriented graphene oxide foam;
[0026] (3) subjecting the vertically oriented graphene oxide foam to a steering process so as to obtain a horizontally oriented graphene oxide foam;
[0027] (4) assembling the horizontally oriented graphene oxide foam, the vertically oriented graphene oxide foam, and the horizontally oriented graphene oxide foam from top to bottom to obtain a composite graphene oxide foam with a sandwich structure;
[0028] (5) carbonizing the composite graphene oxide foam of the sandwich structure to obtain the graphene foam material;
[0029] The density of the horizontally oriented graphene foam is higher than that of the vertically oriented graphene foam, and the density of the material is 30-70 mg cm -3 .
[0030] The method according to the embodiment of the present invention is simple, green, safe and environmentally friendly. The material prepared by the method according to the embodiment of the present invention is composed of a sandwich structure of horizontally oriented graphene foam / vertically oriented graphene foam / horizontally oriented graphene foam, wherein the horizontally oriented graphene foam has a higher density and provides a high in-plane thermal conductivity, and the vertically oriented graphene foam has a lower density, which effectively reduces the density of the overall material while providing a high inter-plane thermal conductivity; high thermal conductivity carbon fibers are introduced into the graphene foam, and the fiber structure is interspersed inside the foam to connect the graphene sheets, effectively improving the mechanical properties of the material. The material prepared by the method according to the embodiment of the present invention has a low density, light weight, and excellent mechanical properties. It can be continuously compressed 10,000 times without substantially changing its morphology, and at the same time has ultra-high in-plane and inter-plane thermal conductivity, and is currently a very high thermal conductivity among foam-type lightweight materials.
[0031] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:
[0032] According to an embodiment of the present invention, the thickness ratio of the horizontally oriented graphene foam to the vertically oriented graphene foam is 1:7-1:10. According to an embodiment of the present invention, this thickness ratio is a better ratio combining light weight and high thermal conductivity. Below this ratio, the proportion of the middle low-density part is too high, the foam is light but the thermal conductivity is reduced; above this ratio, the proportion of the upper and lower horizontally oriented high-density parts is too high, the material has good thermal conductivity, but the density is too high.
[0033] According to an embodiment of the present invention, the density of the horizontally oriented graphene foam is 80-170 mg cm -3 According to an embodiment of the present invention, this density range is a relatively optimal ratio combining light weight and high thermal conductivity. If the density is too high, the material as a whole is too heavy; if the density is too low, the thermal conductivity of the material is reduced.
[0034] According to an embodiment of the present invention, the pore size of the horizontally oriented graphene foam is 5-50 μm. According to an embodiment of the present invention, this pore size range is a better ratio of light weight and high thermal conductivity. If the pore size is too small, the material is too heavy; if the density is too large, the thermal conductivity of the material is reduced.
[0035] According to an embodiment of the present invention, the vertically oriented graphene foam has a density of 30-60 mg cm -3 According to an embodiment of the present invention, this density range is a relatively optimal ratio combining light weight and high thermal conductivity. If the density is too high, the material as a whole is too heavy; if the density is too low, the thermal conductivity of the material is reduced.
[0036] According to an embodiment of the present invention, the pore size of the vertically oriented graphene foam is 30-110 μm. According to an embodiment of the present invention, this pore size range is a better ratio of light weight and high thermal conductivity. If the pore size is too small, the material is too heavy; if the density is too large, the thermal conductivity of the material is reduced.
[0037] According to an embodiment of the present invention, the concentration of the graphene oxide dispersion is 10mg / mL to 15mg / mL. According to an embodiment of the present invention, within this concentration range, graphene oxide is in a flowable slurry state, which can not only ensure the formability during the preparation of graphene foam, but also provide low density and high thermal conductivity at the same time. When the concentration is too low, the graphene oxide dispersion is water-like, has strong fluidity, a large amount of ice crystals formed during the freezing process, uncontrollable growth direction, and the graphene oxide sheets cannot form effective mutual contact, and the resulting oriented structure has poor controllability, and the density is too small and the thermal conductivity is low; when the graphene oxide concentration is too high, it is a non-flowing slurry, and the ice crystal growth process will encounter too many graphene oxide sheets to hinder, and the oriented graphene foam cannot be effectively prepared. And the density of the prepared graphene foam is too large, which affects practical applications.
[0038] According to an embodiment of the present invention, the freezing treatment and drying treatment are performed by pouring the mixed graphene oxide dispersion into a glass beaker, then placing it on a metal plate fixed on the surface of liquid nitrogen for directional freezing, and then transferring it to a freeze dryer for freeze drying.
[0039] According to an embodiment of the present invention, the thickness of the metal plate is 2-5 mm. According to an embodiment of the present invention, if the metal plate is too thin, it is difficult to effectively support sample molding, and if it is too thick, the temperature transmission distance increases, the freezing rate decreases, and the controllability of oriented structure molding becomes worse.
[0040] According to an embodiment of the present invention, the vacuum degree of the freeze dryer is ≤25Pa.
[0041] According to an embodiment of the present invention, the temperature of the freeze dryer is -55°C to -65°C.
[0042] According to an embodiment of the present invention, the freeze-drying time is 72h to 96h.
[0043] According to an embodiment of the present invention, the steering process is performed by laying down a portion of the vertically oriented low-density graphene oxide foam at 90 degrees and applying pressure up and down.
[0044] According to an embodiment of the present invention, the pressure is 5N-20N. According to an embodiment of the present invention, if the pressure is higher than this pressure, the sample is compressed too much and the internal voids are completely destroyed; if the compression is too small, it is difficult to effectively improve the horizontal orientation of the high-density sample, and the horizontal thermal conductivity is limited.
[0045] According to an embodiment of the present invention, the assembly process is carried out at a concentration of 10 mg mL -1 ~15mg mL -1 The reaction was carried out under the condition that graphene oxide solution was used as a binder.
[0046] According to an embodiment of the present invention, the carbonization treatment is carried out at a temperature of 1500-2500°C for 3-5 hours. According to an embodiment of the present invention, the thermal conductivity of graphene is closely related to the degree of reduction. The higher the heat treatment temperature, the greater the degree of reduction and the higher the thermal conductivity. Reduction at 1500°C for 3 hours can achieve a high degree of reduction, and increasing the temperature and time can further increase the degree of reduction. The higher the reduction temperature, the better, but exceeding 2500°C will exceed the temperature that general high-temperature carbonization instruments can withstand, and the cost will increase greatly; thermal reduction can react completely within 5 hours, and further increasing the time will greatly increase the cost. If it is less than 3 hours, the reduction is not complete.
[0047] According to an embodiment of the present invention, the carbonization treatment is performed in an inert atmosphere.
[0048] In another aspect of the present invention, the present invention further provides a method for preparing a graphene foam material. According to an embodiment of the present invention, the method comprises:
[0049] (1) mixing a graphene oxide dispersion and a high thermal conductivity carbon fiber to obtain a mixed graphene oxide dispersion, wherein the concentration of the graphene oxide dispersion is 10 mg / mL to 15 mg / mL;
[0050] (2) placing the mixed graphene oxide dispersion on a metal plate with a thickness of 2-5 mm fixed on the surface of liquid nitrogen for directional freezing, and then transferring it to a freeze dryer for freeze drying to obtain a vertically oriented low-density graphene oxide foam to obtain a vertically oriented graphene oxide foam, wherein the density of the vertically oriented graphene foam is 30-60 mg cm -3 , the pore size of the vertically oriented graphene foam is 30-110 μm, the vacuum degree of the freeze dryer is ≤25 Pa, the temperature of the freeze dryer is -55°C to -65°C, and the freeze drying time is 72h to 96h;
[0051] (3) Lay down part of the vertically oriented low-density graphene oxide foam at 90 degrees, and apply a pressure of 5N-20N up and down to obtain a horizontally oriented graphene oxide foam, wherein the density of the horizontally oriented graphene foam is 80-170 mg cm -3 , the pore size of the horizontally oriented graphene foam is 5-50 μm, and the thickness ratio of the horizontally oriented graphene foam to the vertically oriented graphene foam is 1:7-1:10;
[0052] (4) using a graphene oxide solution with a concentration of 10 mg mL-1 to 15 mg mL-1 as a binder, assembling the horizontally oriented graphene oxide foam, the vertically oriented graphene oxide foam, and the horizontally oriented graphene oxide foam from top to bottom to obtain a composite graphene oxide foam with a sandwich structure;
[0053] (5) Carbonizing the sandwich-structured composite graphene oxide foam at 1500-2500° C. for 3 h to 5 h under an inert atmosphere to obtain the graphene foam material;
[0054] Wherein, the density of the material is 30-70 mg cm -3 .
[0055] The method according to the embodiment of the present invention is simple, green, safe and environmentally friendly. The material prepared by the method according to the embodiment of the present invention is composed of a sandwich structure of horizontally oriented graphene foam / vertically oriented graphene foam / horizontally oriented graphene foam, wherein the horizontally oriented graphene foam has a higher density and provides a high in-plane thermal conductivity, and the vertically oriented graphene foam has a lower density, which effectively reduces the density of the overall material while providing a high inter-plane thermal conductivity; high thermal conductivity carbon fibers are introduced into the graphene foam, and the fiber structure is interspersed inside the foam to connect the graphene sheets, effectively improving the mechanical properties of the material. The material prepared by the method according to the embodiment of the present invention has a low density, light weight, and excellent mechanical properties. It can be continuously compressed 10,000 times without substantially changing its morphology, and at the same time has ultra-high in-plane and inter-plane thermal conductivity, and is currently a very high thermal conductivity among foam-type lightweight materials.
[0056] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:
[0057] According to an embodiment of the present invention, the diameter of the high thermal conductivity carbon fiber is 20-50 μm. According to an embodiment of the present invention, the diameter of the high thermal conductivity carbon fiber will affect its thermal conductivity and dispersibility. In this diameter range, the carbon fiber exhibits excellent thermal conductivity and dispersibility at the same time. For carbon fiber, the smaller the size, the better the dispersibility, but as the diameter decreases, its thermal conductivity will also decrease rapidly. Therefore, below this value, the thermal conductivity of the final material decreases; above this value, the dispersion of the carbon fiber is affected, and the internal structure of the final material is uneven, affecting its overall thermal conductivity, mechanical properties, etc.
[0058] According to an embodiment of the present invention, the length of the high thermal conductivity carbon fiber is 200-1000 μm. According to an embodiment of the present invention, the length of the high thermal conductivity carbon fiber affects its dispersibility in graphene oxide and the thermal conductivity and mechanical properties of the final graphene foam. This length can achieve optimal overall performance. Below this length, it is difficult for carbon fiber to effectively intersperse between graphene layers and form bridges, so the thermal conductivity and mechanical properties of the material deteriorate. Above this length, the dispersibility of carbon fiber and graphene oxide is limited, and it is difficult to form a uniform orientation structure, which affects the integrity and mechanical properties of the final material.
[0059] According to an embodiment of the present invention, the mass ratio of graphene oxide to carbon fiber is 1:5-1:30. According to an embodiment of the present invention, this mass ratio enables the composite material to have complete formability, excellent mechanical properties and thermal conductivity at the same time. Graphite oxide dispersion is prone to cracking during the rapid freezing process of liquid nitrogen. In the initial stage of preparation, carbon fiber and GO are evenly mixed, and carbon fiber can be interspersed between graphene oxide sheets, effectively inhibiting the generation of cracks. If it is higher than this ratio, that is, the amount of carbon fiber is too little, it is difficult to effectively inhibit the generation of cracks during the preparation freezing process; if it is lower than this ratio, that is, the carbon fiber content is too much, the GO solution will be too viscous, the contact between the GO sheets will be reduced, and the integrity and mechanical properties of the material after carbonization will deteriorate.
[0060] According to an embodiment of the present invention, the mixing process is performed in a high-speed ball mill or a stirrer.
[0061] In another aspect of the present invention, the present invention further provides a graphene foam material. According to an embodiment of the present invention, the graphene foam material is prepared according to the above-mentioned method.
[0062] According to an embodiment of the present invention, the present invention proposes a lightweight dual-oriented high thermal conductivity graphene foam material (i.e., the graphene foam material described above), wherein the material is composed of a sandwich-shaped high-density horizontally oriented graphene foam, a low-density vertically oriented graphene foam, a high-density horizontally oriented graphene foam, and high thermal conductivity carbon fibers interspersed therein, with a density of 30-70 mg cm -3 ; Among them, the density of horizontally oriented graphene foam is 80-170 mg cm -3 , pore size of 5-50 μm, vertically oriented graphene foam density of 30-60 mg cm -3 , the pore size is 30-110 μm, and the thickness ratio of horizontally and vertically oriented graphene foam is 1:7-1:10.
[0063] According to an embodiment of the present invention, the present invention proposes a method for preparing the dual-oriented lightweight high thermal conductivity graphene foam material of the present invention, and the method steps are as follows:
[0064] (1) fully mixing a graphene oxide dispersion having a concentration of 10 mg / mL to 15 mg / mL and a high thermal conductivity carbon fiber to obtain a viscous mixed graphene oxide dispersion;
[0065] (2) pouring the mixed graphene oxide dispersion in step 1 into a glass beaker, then placing it on a metal plate fixed on the surface of liquid nitrogen for directional freezing, and then transferring it to a freeze dryer for freeze drying to obtain a vertically oriented low-density graphene oxide foam;
[0066] (3) taking part of the vertically oriented low-density graphene oxide foam, laying it down at 90 degrees to form a horizontally oriented graphene oxide foam, and applying a certain pressure up and down to increase the orientation and density of the graphene oxide;
[0067] (4) Using graphene oxide slurry as a binder, the obtained horizontally oriented and vertically oriented graphene foams are assembled into a sandwich structure.
[0068] (5) Under an inert atmosphere, the sandwich structure composite graphene oxide foam is carbonized at 1500-2500° C. for 3 h to 5 h to obtain a dual-oriented lightweight and high thermal conductivity graphene foam material.
[0069] The diameter of the high thermal conductivity carbon fiber is 20-50 μm and the length is 200-1000 μm; the mixing method is a high-speed ball mill or a stirrer; the mass ratio of graphene oxide to carbon fiber is 1:5-1:30;
[0070] Further, the applied force is 5N-20N;
[0071] Further, the metal plate has a thickness of 2-5 mm;
[0072] Furthermore, the vacuum degree of the freeze dryer is ≤25Pa, the temperature is -55°C to -65°C, and the freeze drying time is 72h to 96h.
[0073] According to the embodiments of the present invention, the present invention has at least one of the following technical effects:
[0074] (1) The material described in the present invention comprises high-density horizontally oriented and low-density vertically oriented graphene foams and high thermal conductivity graphene carbon fibers interspersed therein. The two foam materials with different orientations form a sandwich structure in a high-density / low-density / high-density manner, which not only provides excellent in-plane and inter-plane thermal conductivity, but also effectively reduces the density of the overall material; in addition, the high thermal conductivity carbon fibers are evenly dispersed in the entire graphene foam skeleton, increasing the contact area between graphene sheets and improving the mechanical properties of the high thermal conductivity foam.
[0075] (2) The material described in the present invention has low density, light weight, excellent mechanical properties, and can be compressed continuously for 10,000 times without substantially changing its morphology. It also has ultra-high in-plane and inter-plane thermal conductivity, and has very high thermal conductivity among the current foam-based lightweight materials.
[0076] (3) The method of the present invention is simple, green, safe and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0077] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0078] Figure 1 This is a scanning electron microscope (SEM) image of the high-density horizontally oriented graphene foam material prepared in Example 1;
[0079] Figure 2 A scanning electron microscope (SEM) image of the low-density vertically oriented graphene foam material prepared in Example 1;
[0080] Figure 3 This is a scanning electron microscope (SEM) image of the high-density horizontally oriented graphene foam material prepared in Example 2;
[0081] Figure 4 A scanning electron microscope (SEM) image of the low-density vertically oriented graphene foam material prepared in Example 2;
[0082] Figure 5 This is a scanning electron microscope (SEM) image of the high-density horizontally oriented graphene foam material prepared in Example 3;
[0083] Figure 6 A scanning electron microscope (SEM) image of the low-density vertically oriented graphene foam material prepared in Example 3;
[0084] Figure 7 This is a digital photo of the graphene oxide / carbon fiber composite slurry prepared in Comparative Example 1;
[0085] Figure 8 This is a scanning electron microscope (SEM) image of the high-density horizontally oriented graphene foam material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0086] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0087] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.
[0088] In the following embodiments:
[0089] The graphene oxide dispersion is prepared by the following method: in a 0°C cold trap, 1300mL of concentrated sulfuric acid (98wt%) is placed in a 5000mL beaker (clean and anhydrous), 50g of pre-frozen graphite powder is added during stirring, stirring is continued for 2h, and then 150g of potassium permanganate is slowly added to ensure that the temperature does not exceed 5°C during the process. Then the beaker is placed in a 55°C water bath and stirred for 8-10h to obtain a viscous slurry. The obtained viscous slurry is slowly poured into the stirred excess ice water, and the temperature is kept at no more than 5°C during the water addition process. After cooling to room temperature, 300mL of hydrogen peroxide (30wt%) is added, and the dispersion changes from dark brown to golden yellow. The solution is stirred for 20 minutes to fully mix and react, and then allowed to stand and settle. Discard the supernatant, take 4000mL of deionized water and add it to the lower sediment, stir for 20 minutes and let it settle, discard the supernatant, take another 4000ml of deionized water and add it to the lower sediment, stir, let it settle and discard the supernatant, repeat this process once a day for 7 times, place the sediment obtained in the last dialysis bag for dialysis, change the water every day until the pH of the solution is 7, and then dialyze the sediment at 10000rpm min -1 Centrifuge at a speed of 30 min to remove the impurities in the lower layer and the supernatant to obtain 10 mg mL -1 ~20mgmL -1 The graphene oxide dispersion is calibrated to a certain concentration and set aside.
[0090] Example 1
[0091] (1) Preparation concentration is 12 mg mL -1 Graphene oxide dispersion;
[0092] (2) 50 mL of graphene oxide dispersion and 7 g of carbon fiber were mixed and then heated at 2500 r min. -1 The graphene oxide dispersion and the carbon fiber are fully mixed to obtain a graphene oxide composite slurry;
[0093] (3) The obtained graphene oxide slurry was poured into an uncovered plastic box with a length, width and height of 5 cm×5 cm×1 cm and 5 cm×1 cm×5 cm, respectively, and then placed on the surface of a 5 mm thick stainless steel plate fixed in liquid nitrogen. The plastic box was not in direct contact with the liquid nitrogen, so that the liquid crystal grew vertically from bottom to top and was frozen.
[0094] (4) After freezing for 30 min, it was transferred to a freeze dryer and dried for 72 h to obtain two sizes of vertically oriented graphene oxide foams.
[0095] (5) Rotate the graphene oxide foam of size 5 cm×1 cm×5 cm by 90° to place it horizontally, and turn the pore structure orientation to horizontal; apply a force of 8 N on it to reduce the foam thickness from 1 cm to 2 mm, make the structure denser, and further improve the orientation degree, thereby obtaining a horizontally oriented high-density graphene oxide foam;
[0096] (6) A layer of pure water is evenly sprayed on the upper and lower surfaces of the low-density vertically oriented graphene oxide foam using a spray device to cause the surface layer of the graphene oxide skeleton to partially collapse and become a viscous slurry. Subsequently, the high-density graphene oxide foam is placed on it, and a certain force is applied to tightly combine the two parts to obtain a high-density (1.2 mm)-low-density (10 mm)-high-density (1.2 mm) sandwich structure graphene oxide foam.
[0097] (7) The sandwich structure foam was placed in a high-temperature carbonization furnace, heated to 2000°C in an inert atmosphere, and kept warm for 3 hours to obtain a bi-oriented lightweight and highly thermally conductive graphene foam with a density of 60 kg / m 3 .
[0098] from Figure 1 It can be seen from the SEM image that the high-density graphene foam prepared in this embodiment is horizontally oriented, with a pore size of about 10 μm to 30 μm. Figure 2 It can be seen from the SEM image that the low-density graphene foam prepared in this embodiment is vertically oriented and has a pore size of about 30-80 μm.
[0099] The lightweight and highly thermally conductive graphene foam material prepared in this embodiment was cut into cubes of 1 cm×1 cm×1 cm and subjected to compression mechanical property tests using a universal testing machine. After 10,000 compression cycles, the height dimension loss was less than 10%. The thermal conductivity of the prepared material was tested using a laser thermal conductivity meter, and the in-plane thermal conductivity of the graphene foam material was finally obtained to be 100 W m -1 K -1 The thermal conductivity between the surfaces is 10W m -1 K -1 .
[0100] Example 2
[0101] (1) Preparation concentration is 10 mg mL -1 Graphene oxide dispersion;
[0102] (2) 70 mL of graphene oxide dispersion and 7 g of carbon fiber were mixed, and then rapidly ball milled at a speed of 3000 r / min for 2 min to fully mix the graphene oxide dispersion and the carbon fiber to obtain a graphene oxide composite slurry;
[0103] (3) The obtained graphene oxide slurry was poured into uncovered plastic boxes with a length, width and height of 5 cm×5 cm×1 cm and 5 cm×1 cm×5 cm respectively, and then placed on the surface of a 3 mm thick stainless steel plate fixed in liquid nitrogen. The plastic box was not in direct contact with the liquid nitrogen, so that the liquid crystal grew vertically from bottom to top and was frozen.
[0104] (4) After being frozen for 30 min, the mixture was transferred to a freeze dryer and dried for 72 h to obtain two sizes of vertically oriented graphene oxide foams with a density of 28 mg cm -3 .
[0105] (5) The graphene oxide foam with a size of 5 cm × 1 cm × 5 cm was rotated 90° to place it horizontally, and the pore structure orientation was turned horizontal. A force of 6 N was applied to it, so that the foam thickness was reduced from 1 cm to 2 mm, the structure became dense, and the orientation degree was further improved, resulting in a horizontally oriented high-density graphene oxide foam with a density of 140 mg cm -3 ;
[0106] (6) A layer of pure water is evenly sprayed on the upper and lower surfaces of the low-density vertically oriented graphene oxide foam using a spray device to cause the graphene oxide skeleton to partially collapse and become a viscous slurry. The high-density graphene oxide foam is then placed on it, and a certain force is applied to tightly combine the two parts to obtain a high-density (1 mm)-low-density (10 mm)-high-density (1 mm) sandwich structure graphene oxide foam.
[0107] (7) The sandwich structure foam was placed in a high-temperature carbonization furnace, heated to 2000°C in an inert atmosphere, and kept warm for 3 h to obtain a bi-oriented lightweight and highly thermally conductive graphene foam with a density of 55 kg m -3 .
[0108] from Figure 3 It can be seen from the SEM image that the high-density graphene foam prepared in this embodiment is horizontally oriented, with a pore size of about 20 μm to 50 μm. Figure 4 It can be seen from the SEM image that the low-density graphene foam prepared in this embodiment is vertically oriented and has a pore size of about 80-110 μm.
[0109] The lightweight and highly thermally conductive graphene foam material prepared in this embodiment was cut into cubes of 1 cm × 1 cm × 1 cm and subjected to compression mechanical property tests using a universal testing machine. After 10,000 compression cycles, the dimensional loss in the height direction was less than 10%. The thermal conductivity of the prepared material was tested using a laser thermal conductivity meter, and the in-plane thermal conductivity of the graphene foam material was finally obtained to be 90 W m -1 K -1 The inter-surface thermal conductivity is 8W m -1 K -1 .
[0110] Example 3
[0111] (1) Preparation concentration is 15 mg mL -1 Graphene oxide dispersion;
[0112] (2) 50 mL of graphene oxide dispersion and 7 g of carbon fiber were mixed, and then rapidly ball milled at a speed of 3000 r / min for 2 min to fully mix the graphene oxide dispersion and the carbon fiber to obtain a graphene oxide composite slurry;
[0113] (3) The obtained graphene oxide slurry was poured into uncovered plastic boxes with a length, width and height of 5 cm×5 cm×1 cm and 5 cm×1 cm×5 cm respectively, and then placed on the surface of a 5 mm thick stainless steel plate fixed in liquid nitrogen. The plastic box was not in direct contact with the liquid nitrogen, so that the liquid crystal grew vertically from bottom to top and was frozen.
[0114] (4) After being frozen for 30 min, the mixture was transferred to a freeze dryer and dried for 72 h to obtain two sizes of vertically oriented graphene oxide foams with a density of 28 mg cm -3 .
[0115] (5) Rotate the graphene oxide foam of size 5 cm × 1 cm × 5 cm by 90° so that it is placed horizontally and the pore structure orientation is turned horizontal; apply a force of 10 N on it to reduce the foam thickness from 1 cm to 1 mm, the structure becomes dense, and the orientation degree is further improved, thereby obtaining a horizontally oriented high-density graphene oxide foam;
[0116] (6) A layer of pure water is evenly sprayed on the upper and lower surfaces of the low-density vertically oriented graphene oxide foam using a spray device to cause the graphene oxide skeleton to partially collapse and become a viscous slurry. The high-density graphene oxide foam is then placed on top and a certain force is applied to tightly combine the two parts to obtain a high-density (1 mm)-low-density (9 mm)-high-density (1 mm) sandwich structure graphene oxide foam.
[0117] (7) The sandwich structure foam was placed in a high-temperature carbonization furnace, heated to 2000°C in an inert atmosphere, and kept warm for 3 hours to obtain a bi-oriented lightweight and highly thermally conductive graphene foam with a density of 70 kg / m 3 .
[0118] from Figure 5 It can be seen from the SEM image that the high-density graphene foam prepared in this embodiment is horizontally oriented, with a pore size of about 5 μm to 20 μm. Figure 6 It can be seen from the SEM image that the low-density graphene foam prepared in this embodiment is vertically oriented and has a pore size of about 30-50 μm.
[0119] The lightweight and highly thermally conductive graphene foam material prepared in this embodiment was cut into cubes of 1 cm × 1 cm × 1 cm and subjected to compression mechanical property tests using a universal testing machine. After 10,000 compression cycles, the height dimension loss was less than 10%. The thermal conductivity of the prepared material was tested using a laser thermal conductivity meter, and the in-plane thermal conductivity of the graphene foam material was finally obtained to be 110 W m -1 K -1 The thermal conductivity between the surfaces is 15W m -1 K -1 .
[0120] Comparative Example 1
[0121] (1) Preparation concentration is 15 mg mL -1 Graphene oxide dispersion;
[0122] (2) Mix 50 mL of graphene oxide dispersion and 20 g of carbon fiber, and then heat at 3000 r min. -1 The graphene oxide dispersion and the carbon fiber are fully mixed to obtain a graphene oxide composite slurry;
[0123] (3) The obtained graphene oxide composite slurry was poured into uncovered plastic boxes with a length, width and height of 5 cm×5 cm×1 cm and 5 cm×1 cm×5 cm respectively, and then placed on the surface of a 5 mm thick stainless steel plate fixed in liquid nitrogen. The plastic box was not in direct contact with the liquid nitrogen, so that the liquid crystal grew vertically from bottom to top and was frozen.
[0124] (4) After freezing for 30 min, it was transferred to a freeze dryer and dried for 72 h to obtain two sizes of vertically oriented graphene oxide foams.
[0125] (5) Rotate the graphene oxide foam with a size of 5 cm×1 cm×5 cm by 90° so that it is placed horizontally and the pore structure orientation is turned horizontal; apply a force of 15 N thereon to make the foam dense and the orientation degree further improved, thereby obtaining a horizontally oriented high-density graphene oxide foam;
[0126] (6) A layer of pure water is evenly sprayed on the upper and lower surfaces of the low-density vertically oriented graphene oxide foam using a spray device to cause the graphene oxide skeleton to partially collapse and become a viscous slurry. The high-density graphene oxide foam is then placed on it, and a certain force is applied to tightly combine the two parts to obtain a high-density (5 mm)-low-density (10 mm)-high-density (5 mm) sandwich structure graphene oxide foam.
[0127] (7) The sandwich structure foam was placed in a high-temperature carbonization furnace, heated to 2000°C in an inert atmosphere, and kept warm for 3 h to obtain a bi-oriented lightweight and highly thermally conductive graphene foam with a density of 100 kg m-3 .
[0128] In this embodiment, due to the large amount of carbon fiber added, in step 5, the sample can only be compressed from 1cm to 5mm with a pressure of 15N, and the final sandwich ratio is 5mm:10mm:5mm. Figure 7 It can be seen from the digital photos that the graphene oxide slurry prepared in this embodiment is very viscous and solid, with an obvious layered structure. Figure 8 It can be seen from the SEM image that the high-density graphene foam structure breaks and collapses.
[0129] The lightweight and highly thermally conductive graphene foam material prepared in this embodiment was cut into cubes of 1 cm × 1 cm × 1 cm and subjected to compression mechanical property tests using a universal testing machine. After 10,000 compression cycles, the height dimension loss exceeded 50%. The thermal conductivity of the prepared material was tested using a laser thermal conductivity meter, and the in-plane thermal conductivity of the graphene foam material was finally obtained to be 30 W m -1 K -1 The inter-surface thermal conductivity is 6W m -1 K -1 .
[0130] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0131] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A graphene foam material, characterized in that: include: Bottom layer, middle layer and surface layer, The bottom layer is horizontally oriented graphene foam; The middle layer is vertically oriented graphene foam; The surface layer is horizontally oriented graphene foam; The density of the horizontally oriented graphene foam is higher than the density of the vertically oriented graphene foam; The bottom layer, the middle layer and the surface layer all contain high thermal conductivity carbon fibers; The density of the material is 30-70 mg cm -3 .
2. The graphene foam material according to claim 1, characterized in that: The thickness ratio of the horizontally oriented graphene foam to the vertically oriented graphene foam is 1:7-1:10; Optionally, the density of the horizontally oriented graphene foam is 80-170 mg cm -3 ; Optionally, the pore size of the horizontally oriented graphene foam is 5-50 μm; Optionally, the vertically oriented graphene foam has a density of 30-60 mg cm -3 ; Optionally, the vertically oriented graphene foam has a pore size of 30-110 μm; Optionally, the diameter of the high thermal conductivity carbon fiber is 20-50 μm; Optionally, the length of the high thermal conductivity carbon fiber is 200-1000 μm; Optionally, the graphene is present in the form of graphene oxide; Optionally, the mass ratio of the graphene oxide to the carbon fiber is 1:5-1:
30.
3. A method for preparing a graphene foam material, characterized in that: (1) mixing a graphene oxide dispersion and a high thermal conductivity carbon fiber to obtain a mixed graphene oxide dispersion; (2) freezing and drying the mixed graphene oxide dispersion to obtain vertically oriented graphene oxide foam; (3) subjecting the vertically oriented graphene oxide foam to a steering process so as to obtain a horizontally oriented graphene oxide foam; (4) assembling the horizontally oriented graphene oxide foam, the vertically oriented graphene oxide foam, and the horizontally oriented graphene oxide foam from top to bottom to obtain a composite graphene oxide foam with a sandwich structure; (5) carbonizing the composite graphene oxide foam of the sandwich structure to obtain the graphene foam material; The density of the horizontally oriented graphene foam is higher than that of the vertically oriented graphene foam, and the density of the material is 30-70 mg cm -3 .
4. The method according to claim 3, characterized in that The thickness ratio of the horizontally oriented graphene foam to the vertically oriented graphene foam is 1:7-1:10; Optionally, the density of the horizontally oriented graphene foam is 80-170 mg cm -3 ; Optionally, the pore size of the horizontally oriented graphene foam is 5-50 μm; Optionally, the vertically oriented graphene foam has a density of 30-60 mg cm -3 ; Optionally, the vertically oriented graphene foam has a pore size of 30-110 μm.
5. The method according to claim 3 or 4, characterized in that: The concentration of the graphene oxide dispersion is 10 mg / mL to 15 mg / mL; Optionally, the freezing treatment and drying treatment are performed by pouring the mixed graphene oxide dispersion into a glass beaker, placing it on a metal plate fixed on the surface of liquid nitrogen for directional freezing, and then transferring it to a freeze dryer for freeze drying; Optionally, the metal plate has a thickness of 2-5 mm; Optionally, the vacuum degree of the freeze dryer is ≤25Pa; Optionally, the temperature of the freeze dryer is -55°C to -65°C; Optionally, the freeze-drying time is 72 h to 96 h.
6. The method according to any one of claims 3 to 5, characterized in that: The steering process is performed by laying down a portion of the vertically oriented low-density graphene oxide foam at 90 degrees and applying pressure up and down; Optionally, the pressure is 5N-20N.
7. The method according to any one of claims 3 to 5, characterized in that: The assembly treatment was performed at a concentration of 10 mg mL -1 ~15mg mL -1 The graphene oxide solution is used as a binder; Optionally, the carbonization treatment is carried out at a temperature of 1500-2500° C. for 3-5 hours; Optionally, the carbonization treatment is performed in an inert atmosphere.
8. A method for preparing a graphene foam material, characterized in that: (1) mixing a graphene oxide dispersion and a high thermal conductivity carbon fiber to obtain a mixed graphene oxide dispersion, wherein the concentration of the graphene oxide dispersion is 10 mg / mL to 15 mg / mL; (2) placing the mixed graphene oxide dispersion on a metal plate with a thickness of 2-5 mm fixed on the surface of liquid nitrogen for directional freezing, and then transferring it to a freeze dryer for freeze drying to obtain a vertically oriented low-density graphene oxide foam to obtain a vertically oriented graphene oxide foam, wherein the density of the vertically oriented graphene foam is 30-60 mg cm -3 , the pore size of the vertically oriented graphene foam is 30-110 μm, the vacuum degree of the freeze dryer is ≤25 Pa, the temperature of the freeze dryer is -55°C to -65°C, and the freeze drying time is 72h to 96h; (3) Lay down part of the vertically oriented low-density graphene oxide foam at 90 degrees, and apply a pressure of 5N-20N up and down to obtain a horizontally oriented graphene oxide foam, wherein the density of the horizontally oriented graphene foam is 80-170 mg cm -3 , the pore size of the horizontally oriented graphene foam is 5-50 μm, and the thickness ratio of the horizontally oriented graphene foam to the vertically oriented graphene foam is 1:7-1:10; (4) using a graphene oxide solution with a concentration of 10 mg mL-1 to 15 mg mL-1 as a binder, assembling the horizontally oriented graphene oxide foam, the vertically oriented graphene oxide foam, and the horizontally oriented graphene oxide foam from top to bottom to obtain a composite graphene oxide foam with a sandwich structure; (5) Carbonizing the sandwich-structured composite graphene oxide foam at 1500-2500° C. for 3 h to 5 h under an inert atmosphere to obtain the graphene foam material; Wherein, the density of the material is 30-70 mg cm -3 .
9. The method according to any one of claims 3 to 8, characterized in that: The diameter of the high thermal conductivity carbon fiber is 20-50 μm; Optionally, the high thermal conductivity carbon fiber has a length of 200-1000 μm; Optionally, the mass ratio of graphene oxide to carbon fiber is 1:5-1:30; Optionally, the mixing process is carried out in a high-speed ball mill or a stirrer.
10. A graphene foam material, characterized in that: The graphene foam material is prepared according to the method according to any one of claims 3-8.
Citation Information
Patent Citations
High-strength and high-heat-conduction three-dimensional graphene heat dissipating material and preparation method thereof
CN106967392A
Method for preparing carbon fiber reinforced graphene foam block and related product
CN114890815A
Graphene foam block, heat-conducting sheet, gasket, arrangement device and preparation method
CN115057432A
Graphene composite longitudinal heat-conducting film and preparation method thereof
CN116922877A
Mesophase pitch-based carbon fiber / graphene / epoxy resin high-thermal-conductivity composite material based on vertical orientation and preparation method thereof