Tungsten trioxide powder and preparation method and application thereof

The preparation of tungsten trioxide powder by hydrothermal method using organic acid regulators solves the problems of complex preparation process and environmental pollution in the prior art, realizes cost reduction and performance improvement, and provides adsorption, photocatalytic and gas-sensitive materials. Wide application.

CN118954603APending Publication Date: 2024-11-15SHANDONG JIANZHU UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411142031.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the operation process of using sodium tungstate and concentrated acid to prepare tungsten trioxide powder is complex, costly and prone to environmental pollution.

Method used

Using organic acid as morphological regulator, tungsten powder and hydrogen peroxide aqueous solution were mixed by hydrothermal method, and a hydrothermal reaction was carried out to prepare tungsten trioxide powder, which simplified the preparation process, reduced production costs, and reduced environmental pollution.

Benefits of technology

The preparation of tungsten trioxide powder with different morphology has been achieved, which reduces production costs, simplifies operating procedures, and reduces environmental pollution, providing application prospects in adsorption, photocatalytic and gas-sensitive materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954603A_ABST
    Figure CN118954603A_ABST
Patent Text Reader

Abstract

The invention provides tungsten trioxide powder as well as a preparation method and application thereof, and relates to the technical field of powder materials. The preparation method of the tungsten trioxide powder provided by the invention comprises the following steps: dissolving tungsten powder in a hydrogen peroxide aqueous solution to obtain a tungsten-containing solution; and mixing the tungsten-containing solution with an organic acid aqueous solution, and carrying out a hydrothermal reaction to obtain the tungsten trioxide powder. Tungsten powder is dissolved in a hydrogen peroxide aqueous solution to form peroxytungstate, then organic acid is used as a morphology regulator to convert peroxytungstic acid into tungsten trioxide with different morphologies, and the organic acid plays a role of a'soft template '; meanwhile, the organic acid has an association effect of a hydrogen bond in an aqueous solution, so that the morphology of the tungsten trioxide powder can be controlled. The tungsten trioxide powder with different morphologies prepared by the method has different specific surface areas, provides different positions of active sites for catalytic reaction, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder materials, and specifically relates to tungsten trioxide powder and a preparation method and application thereof. Background Art

[0002] Tungsten trioxide (WO3) is one of the few semiconductor oxides that can easily achieve quantum size effects. It has been widely studied and applied in the fields of photochromism, electrochromism, field emission electronic materials, photocatalytic degradation of organic pollutants, photoelectrocatalytic decomposition of water to produce hydrogen, gas-sensitive materials, adsorption, lithium-ion batteries and supercapacitors. Studies have shown that there is a direct relationship between the different microscopic morphologies of nanostructured materials and their performance. The controllable preparation of nanomaterials with different morphologies is of great significance for regulating their performance. In the existing technology, sodium tungstate and concentrated acid are usually used as raw materials to prepare tungsten oxide powder. Not only is the operation process complicated, but the amount of concentrated acid (such as concentrated hydrochloric acid and concentrated nitric acid) used is large, which is easy to cause environmental pollution and has high costs. Summary of the invention

[0003] The purpose of the present invention is to provide a tungsten trioxide powder and a preparation method and application thereof. The present invention adopts an organic acid as a morphology regulator and directly uses a hydrothermal method to prepare tungsten trioxide powders with different morphologies. The preparation method is simple, the production cost is lower, and the pollution to the environment is reduced.

[0004] In order to achieve the purpose of the present invention, the present invention provides the following technical solutions: A method for preparing tungsten trioxide powder comprises the following steps: dissolving tungsten powder in a hydrogen peroxide solution to obtain a tungsten-containing solution; The tungsten-containing solution and the organic acid aqueous solution are mixed and subjected to a hydrothermal reaction to obtain the tungsten trioxide powder.

[0005] Preferably, the particle size of the tungsten powder is 0.05-5 μm.

[0006] Preferably, the mass fraction of the aqueous hydrogen peroxide solution is 30-60%; the dosage ratio of the tungsten powder to the aqueous hydrogen peroxide solution is 0.5-1.5 g:5-20 mL.

[0007] Preferably, the organic acid in the organic acid aqueous solution includes one or more of tartaric acid, oxalic acid and citric acid.

[0008] Preferably, the concentration of the organic acid aqueous solution is 1.6-50 g / L; the mass ratio of the tungsten powder to the organic acid in the organic acid aqueous solution is 0.5-3:0.5-9.

[0009] Preferably, after the tungsten-containing solution and the organic acid aqueous solution are mixed, the pH value is adjusted to 1-6.

[0010] Preferably, the reagent used to adjust the pH value includes one or more of dilute hydrochloric acid, nitric acid and sulfuric acid.

[0011] Preferably, the temperature of the hydrothermal reaction is 160-200° C., and the time is 8-36 hours.

[0012] The present invention also provides tungsten trioxide powder prepared by the preparation method described in the above technical solution, wherein the structure of the tungsten trioxide powder includes one or more of one-dimensional nanowires, two-dimensional nanosheets and three-dimensional flower-shaped nanostructures.

[0013] The present invention also provides the use of the tungsten trioxide powder described in the above technical solution in adsorption, photocatalytic degradation of pollutants, electrochromic or gas-sensitive materials.

[0014] The present invention provides a method for preparing tungsten trioxide powder, comprising the following steps: dissolving tungsten powder in a hydrogen peroxide aqueous solution to obtain a tungsten-containing solution; mixing the tungsten-containing solution and an organic acid aqueous solution, and performing a hydrothermal reaction to obtain the tungsten trioxide powder. In the present invention, tungsten powder is dissolved in a hydrogen peroxide aqueous solution to form pertungstic acid, and then the pertungstic acid is converted into tungsten trioxide by an organic acid, wherein the organic acid plays the role of a "soft template"; at the same time, the organic acid has a hydrogen bond association effect in the aqueous solution, and can control the morphology of the tungsten trioxide powder.

[0015] Furthermore, different organic acids in the present invention have different molecular structures. When the organic acid is oxalic acid, the structure of the prepared tungsten trioxide powder is a one-dimensional nanowire; when the organic acid is citric acid, the morphology of the prepared tungsten trioxide powder is a structural nanosheet; when the organic acid is tartaric acid, the structure of the prepared tungsten trioxide powder is a three-dimensional flower-like nanostructure.

[0016] The present invention also provides tungsten trioxide powder prepared by the preparation method described in the above technical solution, wherein WO3 with different morphologies has different specific surface areas, and the positions of active sites provided for catalytic reactions are different; wherein the two-dimensional sheet structure is conducive to the transmission of photogenerated electrons and holes, has high photocatalytic degradation performance of organic pollutants, and has broad application prospects in the field of photocatalytic environmental treatment of organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0018] Figure 1This is the SEM image of WO3 powder prepared in Example 1; Figure 2 This is the SEM image of WO3 powder prepared in Example 2; Figure 3 This is the SEM image of WO3 powder prepared in Example 3; Figure 4 XRD patterns of WO3 powders prepared in Examples 1 to 3; Figure 5 The nitrogen adsorption-desorption curves of WO3 powder prepared in Examples 1 to 3 are shown. DETAILED DESCRIPTION

[0019] The present invention provides a method for preparing tungsten trioxide powder, comprising the following steps: dissolving tungsten powder in a hydrogen peroxide solution to obtain a tungsten-containing solution; The tungsten-containing solution and the organic acid aqueous solution are mixed and subjected to a hydrothermal reaction to obtain the tungsten trioxide powder.

[0020] In the present invention, unless otherwise specified, all preparation raw materials are preferably commercially available products well known to those skilled in the art.

[0021] The present invention dissolves tungsten powder in a hydrogen peroxide solution to obtain a tungsten-containing solution. In the present invention, the particle size of the tungsten powder is preferably 0.05-5 μm, more preferably 0.1-2 μm, and most preferably 0.2-1 μm.

[0022] In the present invention, the mass fraction of the aqueous hydrogen peroxide solution is preferably 30-60%, more preferably 40-50%. In the present invention, the dosage ratio of the tungsten powder to the aqueous hydrogen peroxide solution is preferably 0.5-1.5 g:5-20 mL, more preferably 0.9-1.2 g:5-15 mL.

[0023] In the present invention, a pertungstic acid solution is obtained by dissolving tungsten powder in an aqueous hydrogen peroxide solution.

[0024] The present invention has no special limitation on the dissolution conditions, as long as the tungsten powder is completely dissolved in hydrogen peroxide.

[0025] After obtaining the tungsten-containing solution, the present invention mixes the tungsten-containing solution and an organic acid aqueous solution, performs a hydrothermal reaction, and obtains the tungsten trioxide powder. In the present invention, the organic acid in the organic acid aqueous solution preferably includes one or more of tartaric acid, oxalic acid, and citric acid. In the present invention, the concentration of the organic acid aqueous solution is preferably 1.6~50g / L, more preferably 10~40g / L, and further preferably 23~30g / L. In the present invention, the mass ratio of the tungsten powder and the organic acid in the organic acid aqueous solution is preferably 0.5~3:0.5~9, more preferably 0.9~1.2:0.6~2.4, and further preferably 1:1.4. In the present invention, the organic acid plays the role of a "soft template" in the process of converting pertungstic acid into tungsten trioxide. At the same time, the organic acid has a hydrogen bond association in the aqueous solution, which plays a role in controlling the morphology of the nanoparticles. Furthermore, different organic acids in the present invention have different molecular structures. When the organic acid is oxalic acid, the structure of the prepared tungsten trioxide powder is a one-dimensional nanowire; when the organic acid is citric acid, the structure of the prepared tungsten trioxide powder is a two-dimensional nanosheet; when the organic acid is tartaric acid, the structure of the prepared tungsten trioxide powder is a three-dimensional flower-like nanostructure.

[0026] The present invention has no particular limitation on the manner and conditions for mixing the tungsten-containing solution and the organic acid, and any manner and conditions familiar to those skilled in the art may be used.

[0027] In the present invention, the pH value of the mixed solution obtained by mixing the tungsten-containing solution and the organic acid aqueous solution is preferably adjusted to 1 to 6, more preferably 2 to 4. In the present invention, the reagent used to adjust the pH value includes one or more of dilute hydrochloric acid, nitric acid and sulfuric acid; the concentration of the reagent used to adjust the pH value is preferably 0.01 to 0.05 mol / L.

[0028] In the present invention, the temperature of the hydrothermal reaction is preferably 160-200°C, more preferably 180-190°C; the time is preferably 8-36h, more preferably 12-24h, and further preferably 12-15h. In the present invention, the hydrothermal reaction is preferably carried out in a hydrothermal kettle; the inner lining of the hydrothermal kettle is preferably a polytetrafluoroethylene lining.

[0029] In the present invention, after the hydrothermal reaction, the hydrothermal reaction product is preferably washed and dried in sequence. In the present invention, the reagents used for the washing are preferably deionized water and ethanol; the number of washings is preferably 2 to 4 times, more preferably 3 times. The present invention does not specifically limit the drying method, and a drying method well known to those skilled in the art can be used.

[0030] The present invention also provides tungsten trioxide powder prepared by the preparation method described in the above technical solution, wherein the structure of the tungsten trioxide powder includes one or more of one-dimensional nanowires, two-dimensional nanosheets and three-dimensional flower-like nanostructures, more preferably two-dimensional nanosheets.

[0031] The present invention also provides the use of the tungsten trioxide powder described in the above technical solution in adsorption, photocatalytic degradation of pollutants, electrochromic or gas-sensitive materials.

[0032] In order to further illustrate the present invention, the tungsten trioxide powder provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and examples, but they should not be understood as limiting the scope of protection of the present invention.

[0033] Example 1

[0034] 0.9 g of tungsten powder with a particle size of 50 nm was dissolved in 5 mL of H2O2 aqueous solution (mass fraction 30%) to obtain a clear and transparent tungsten-containing solution; The above tungsten-containing solution was diluted to 60 mL by adding deionized water, and then 0.6 g of oxalic acid aqueous solution was added. After stirring for 60 min, 0.05 mol / L H2SO4 was used to adjust the pH value of the solution to 2.0 to obtain a mixed solution. The mixed solution was transferred into a hydrothermal kettle with a polytetrafluoroethylene liner, and the hydrothermal reaction was carried out at 180°C for 12 h. After cooling to room temperature, the hydrothermal reaction product was centrifuged and filtered, washed with deionized water and ethanol for 3 times, and dried in an oven to obtain tungsten trioxide powder.

[0035] Example 2

[0036] 1.2 g of tungsten powder with a particle size of 100 nm was dissolved in 20 mL of H2O2 aqueous solution (mass fraction 30%) to obtain a clear and transparent tungsten-containing solution; The above tungsten-containing solution was diluted to 60 mL by adding deionized water, and then 2.4 g of citric acid aqueous solution was added. After stirring for 60 min, 0.01 mol / L HCl was used to adjust the pH value of the solution to 4.0 to obtain a mixed solution. The mixed solution was transferred into a hydrothermal autoclave with a polytetrafluoroethylene liner, and the hydrothermal reaction was carried out at 180 ° C for 24 h. After cooling to room temperature, the hydrothermal reaction product was centrifuged and filtered, washed with deionized water and ethanol for 3 times, and dried in an oven to obtain tungsten trioxide powder.

[0037] Example 3

[0038] 1.0 g of tungsten powder with a particle size of 200 nm was dissolved in 15 mL of H2O2 aqueous solution (mass fraction 30%) to obtain a clear and transparent tungsten-containing solution; The above tungsten-containing solution was diluted to 60 mL by adding deionized water, and then 1.4 g of tartaric acid aqueous solution was added. After stirring for 60 min, 0.01 mol / L HNO3 was used to adjust the pH value of the solution to 4.0 to obtain a mixed solution. The mixed solution was transferred into a hydrothermal kettle with a polytetrafluoroethylene liner, and the hydrothermal reaction was carried out at 180 ° C for 16 h. After cooling to room temperature, the hydrothermal reaction product was centrifuged and filtered, washed with deionized water and ethanol for 3 times, and dried in an oven to obtain tungsten trioxide powder.

[0039] Test Case

[0040] Figure 1 This is the SEM image of the WO3 powder prepared in Example 1. Figure 1 It can be seen that when the organic acid is oxalic acid, the morphology of the prepared tungsten trioxide powder is one-dimensional nanowires.

[0041] Figure 2 This is the SEM image of WO3 powder prepared in Example 2. Figure 2 It can be seen that when the organic acid is citric acid, the morphology of the prepared tungsten trioxide powder is a two-dimensional nanosheet.

[0042] Figure 3 This is the SEM image of WO3 powder prepared in Example 3. Figure 3 It can be seen that when the organic acid is tartaric acid, the morphology of the prepared tungsten trioxide powder is a three-dimensional flower-like nanostructure.

[0043] Figure 4 The XRD patterns of the WO3 powders prepared in Examples 1 to 3 are as follows: Figure 4 It can be seen that the tungsten trioxide powders prepared by using three organic acids as morphology regulators have the same phase structure, which is WO3·0.5H2O.

[0044] Figure 5 is a nitrogen adsorption-desorption curve of WO3 powder prepared in Examples 1 to 3; Figure 5 It can be seen that the tungsten trioxide powders prepared by using three kinds of organic acids as morphology regulators have different specific surface areas and pore structures, among which the two-dimensional sheet structure tungsten trioxide has a higher specific surface area.

[0045] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing tungsten trioxide powder, characterized in that: The following steps are involved: dissolving tungsten powder in a hydrogen peroxide solution to obtain a tungsten-containing solution; The tungsten-containing solution and the organic acid aqueous solution are mixed and subjected to a hydrothermal reaction to obtain the tungsten trioxide powder.

2. The preparation method according to claim 1, characterized in that: The particle size of the tungsten powder is 0.05-5 μm.

3. The preparation method according to claim 1 or 2, characterized in that: The mass fraction of the aqueous hydrogen peroxide solution is 30-60%; the dosage ratio of the tungsten powder to the aqueous hydrogen peroxide solution is 0.5-1.5 g:5-20 mL.

4. The preparation method according to claim 1, characterized in that: The organic acid in the organic acid aqueous solution includes one or more of tartaric acid, oxalic acid and citric acid.

5. The preparation method according to claim 1 or 4, characterized in that: The concentration of the organic acid aqueous solution is 1.6-50 g / L; the mass ratio of the tungsten powder to the organic acid in the organic acid aqueous solution is 0.5-3:0.5-9.

6. The preparation method according to claim 1, characterized in that: After the tungsten-containing solution and the organic acid aqueous solution are mixed, the pH value is adjusted to 1-6.

7. The preparation method according to claim 6, characterized in that: The reagent used to adjust the pH value includes one or more of dilute hydrochloric acid, nitric acid and sulfuric acid.

8. The preparation method according to claim 1, 6 or 7, characterized in that: The temperature of the hydrothermal reaction is 160-200° C., and the time is 8-36 hours.

9. The tungsten trioxide powder prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The structure of the tungsten trioxide powder includes one or more of a one-dimensional nanowire, a two-dimensional nanosheet and a three-dimensional flower-shaped nanostructure.

10. Use of the tungsten trioxide powder according to claim 9 in adsorption, photocatalytic degradation of pollutants, electrochromic or gas-sensitive materials.