High-gelling-property phosphoaluminate cement prepared from inferior raw materials and preparation method of high-gelling-property phosphoaluminate cement
Through specific calcining process and raw material ratio, the content of calcium aluminate and calcium aluminate is improved, and the problems of deterioration of cementitious cement and the use of inferior raw materials are solved, and high gelability and excellent mechanical properties are achieved The preparation of aluminate cement has wider application and meets environmental protection and carbon reduction requirements.
Patent Information
- Application Number
- CN202411408947.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-15
AI Technical Summary
During the modification process, the existing aluminate cement has reduced the mineral phase content of calcium aluminate and calcium aluminate, resulting in a decrease in gelability. Due to the shortage of high-quality raw materials, inferior raw materials need to be used, and the impurity components affect the preparation of cement. , reduce gelling activity.
Use low-quality raw materials such as low-grade limestone, phosphate tailings and aluminum ash to prepare phosphate cement through specific calcining processes (including crushing, drying, grinding and mixing, heating and insulation and air-cooling cooling) to improve phosphate aluminate cement. The content and gelling activity of calcium and calcium aluminate form a mineral phase with high content of calcium aluminate and dicalcium silicate, improving the impermeability and corrosion resistance of cement.
Improve the gelability and early strength of calcium aluminate cement, enhance the anti-seepage and corrosion resistance, reduce the carbonization reaction of hydration products, prolong the mechanical properties in the hydration process, and have wider applicability and reduce Solid waste pollution is in line with the carbon reduction policy.
Smart Images

Figure CN118954989A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement materials, and in particular relates to a high-gelling aluminophosphate cement prepared by using inferior raw materials and a method thereof. Background Art
[0002] Calcium phosphate cement is a biocement material with high long-term strength and stable hydration products (hydroxyphosphate rock powder). However, its main mineral, tricalcium phosphate, reacts slowly with water at room temperature and has low early strength. Li Shiqun et al. used the partition test method in the CaO-Al2O3-P2O5 ternary phase diagram to explore and synthesized a hydraulic material containing a new phase by the sol-gel method. Its mineral composition is Li Hu (LHss) solid solution phase (considered to be aluminophosphate solid solution), monocalcium aluminate (CA), dicalcium aluminate (C2A), tricalcium phosphate (C3P) and a small amount of glass phase, which was later called phosphate aluminate cement. This new type of cement has excellent impermeability, sulfate erosion resistance, high temperature resistance, excellent frost resistance, repair performance and steel protection performance.
[0003] At present, the literature studies have modified phosphate aluminate cement to produce high-iron phosphate aluminate cement clinker, C4A3$ type phosphate aluminate cement clinker and phosphate aluminate cement clinker containing Q / P phase. The patent with publication number CN104140216B discloses a phosphate aluminate cement clinker, which is fired at 1300℃~1370℃ to produce phosphate aluminate cement clinker with high iron calcium aluminate content, and the mineral composition is LHss24.6%~48.3%, CA (1-Y) (P Y ) 16.5~49.3%, CP (1-Z) (A Z )12.6%~14.6%, C2A x F 1-x (0.3≤x≤0.7) 12.1%~20.6%, the rest is glass phase and other impurities. The patent with publication number CN108059377A discloses a C4A3$ type aluminophosphate cement clinker, the firing temperature is 1350℃~1400℃, the mineral phase composition percentage content is: 35%~45% calcium aluminophosphate, 30%~40% calcium sulfoaluminate, 5%~10% calcium aluminoferrate, 15%~25% calcium phosphate, and 1%~10% intermediate phase. The patent with publication number CN113185161A discloses a phosphate aluminophosphate cement clinker containing Q / P phase, the mineral composition is 5%~40% Q / P phase, 30%~60% calcium aluminophosphate, 20%~50% calcium aluminate, 5%~10% tricalcium phosphate, and 0-10% tetracalcium aluminoferrate.
[0004] A lot of modification research has been conducted on phosphate aluminate cement, and C4A3$, Q / P, C4AF mineral phases have been generated, but at the same time, the mineral phase content of calcium phosphate aluminate and calcium aluminate has been reduced, which has reduced the gelling property of phosphate aluminate cement. At the same time, due to the shortage of high-quality raw materials, it is necessary to use inferior raw materials including low-grade limestone, phosphorus tailings, aluminum ash, etc. to produce phosphate aluminate cement. However, the impurities in the inferior raw materials will affect the preparation of phosphate aluminate cement and reduce the gelling activity of phosphate aluminate. Summary of the invention
[0005] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for preparing high-cementitious phosphate aluminate cement using inferior raw materials in view of the shortcomings of the prior art, thereby increasing the content of calcium phosphate aluminate mineral phase and the gelling activity, and promoting the production and application of calcium phosphate aluminate cement.
[0006] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is as follows: A method for preparing high-gelling aluminophosphate cement using inferior raw materials comprises the following steps: (1) Crushing, drying and grinding calcium raw materials, phosphate rock and aluminum raw materials together, and mixing and homogenizing to obtain raw materials; wherein the raw materials have a weight percentage of: 35-40% CaO, 45-60% Al2O3, 5-10% P2O5, 5-10% SiO2, and other impurities of 1-10%; (2) heating the raw material obtained in step (1) to 900-950° C. at a heating rate of 5-10° C. / min, keeping the temperature for 30 min, and then heating the raw material to 1460-1530° C. at a heating rate of 5-10° C. / min, keeping the temperature for 60-120 min, to obtain a calcined clinker block; (3) The calcined clinker block obtained in step (2) is cooled by air cooling and then ground to obtain a calcined clinker block.
[0007] Specifically, the calcium raw material includes at least one of low-grade limestone, quicklime or slaked lime, preferably low-grade limestone, wherein the mass percentage of CaO is 40-50%.
[0008] Specifically, the phosphate rock includes at least one of phosphate rock powder and phosphate rock tailings, preferably phosphate rock powder, which includes the following components in percentage by mass: 20-25% P2O5, 40-48% CaO, and 5-10% SiO2.
[0009] Specifically, the aluminum raw material includes at least one of aluminum ash, coal gangue, and fly ash, preferably aluminum ash, which includes the following components in percentage by mass: 5-9% MgO, 75-85% Al2O3, and 5-8% SiO2.
[0010] Preferably, in step (1), the calcium raw material, phosphate rock and aluminum raw material are mixed in a mass ratio of (15-25): (35-45): (35-45) to obtain raw material.
[0011] Preferably, in step (1), other impurities in the raw material contain at least MgO and SO3.
[0012] Furthermore, in step (1), the raw material is also mixed with 0.5-1.5% by mass of CaF2.
[0013] Preferably, in step (1), the calcium raw material, phosphate rock and aluminum raw material are ground to 200-400 mesh and then fully mixed with CaF2.
[0014] Furthermore, the aluminophosphate cement prepared by the above preparation method is also within the protection scope of the present invention.
[0015] Specifically, the mineral composition percentage of the phosphate aluminate cement prepared by the present invention is as follows: 45-60% CAP, 15-25% CA2, 10-20% C2AS, 2-10% C2S, 3-15% MA, and 1-10% other mineral phases.
[0016] Compared with the prior art, the present invention has the following beneficial effects: First, the method for preparing phosphate aluminate cement clinker provided by the present invention is to generate the cement clinker by calcining once at a relatively high temperature (1460-1530°C), wherein the content of calcium phosphate aluminate and calcium aluminate ore phase is high (50%-85%), and the gelling performance advantages of calcium phosphate aluminate and calcium aluminate in calcium phosphate aluminate cement can be fully utilized. Since the calcium phosphate aluminate and calcium aluminate phases are hydrated relatively quickly in the early stage, the cement matrix structure develops relatively densely, and thus has excellent impermeability and corrosion resistance; at the same time, the main hydration products of phosphate aluminate cement, calcium phosphate aluminate gel and hydroxyapatite, are relatively stable at high temperatures and are not easy to decompose, so that the phosphate aluminate cement has good high temperature resistance; in addition, the hydration product of phosphate aluminate cement, calcium hydroxide, is produced in a low amount and is not easy to react with CO2 for carbonization, so that the phosphate aluminate cement has excellent CO2 corrosion resistance.
[0017] Second, the present invention prepares phosphate aluminate cement by calcining at a relatively high temperature, so that the Si element introduced into the inferior raw materials (including low-grade limestone, aluminum ash, phosphorus tailings, etc.) combines with the Ca element to generate dicalcium silicate (C2S) with high activity, and reduces the generation of calcium aluminum feldspar (C2AS) with low hydration activity. At the same time, the generation of dicalcium silicate phase is conducive to the development of the later strength of phosphate aluminate cement; in addition, a certain amount of SiO2 is allowed in the raw materials, so the raw material selection is more extensive, which is more conducive to the use of inferior raw materials.
[0018] Third, the phosphate cement prepared by the present invention using inferior raw materials has high gelling property, and the 3d compressive strength is as high as 95MPa, and the 28d compressive strength is as high as 105MPa. The formation of high-content calcium phosphate aluminate and calcium aluminate mineral phase promotes the development of early mechanical properties of phosphate cement, while the formation of dicalcium silicate is conducive to the development of late mechanical properties of phosphate cement, so that phosphate cement has good mechanical properties throughout the entire hydration process.
[0019] Fourth, the present invention uses trace components such as MgO and SO3 in inferior raw materials, which can act as mineralizers, are beneficial to the generation of clinker liquid phase, reduce the burning temperature of clinker to a certain extent, and are beneficial to the formation of high-temperature mineral phase calcium phosphate aluminate. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0021] Figure 1 The XRD analysis diagram of the phosphate aluminate cement clinker minerals of Examples 1 to 4. DETAILED DESCRIPTION
[0022] The present invention can be better understood with reference to the following examples.
[0023] The present invention uses low-grade limestone, aluminum ash and phosphate ore tailings as raw materials, and their chemical compositions are shown in Table 1.
[0024] Table 1 Chemical composition of raw materials (wt / %)
[0025] The raw material proportions in Examples 1-4 are shown in Table 2.
[0026] Table 2 Raw material ratio of phosphate aluminate cement (wt / %) Example 1
[0027] The production method of high-gelling aluminophosphate cement using a low-quality raw material in Example 1 is as follows: The low-grade limestone, phosphate tailings, etc. are crushed, and the raw materials are ground by planetary mill to a fineness of 74μm square hole sieve with a sieve residue of <5%. Raw material ratio: 19.5% limestone, 40.45% phosphate tailings, 40.05% aluminum ash, and the ingredients are mixed by a measuring scale. The chemical composition of each raw material is shown in Table 1. 1% CaF2 is added to the weighed raw materials and mixed to prepare raw material powder. Add 5% water by weight to the raw material powder, mix evenly, press it into a test cake of Ф×8mm (thickness) with a press, and dry it in a dryer at 105℃. The test cake is placed in a high-temperature furnace for calcination, and the heating rate is 10℃ / min. After the temperature reaches 950℃, keep it warm for half an hour, and then heat it to 1530℃ and keep it warm for 2 hours. Take out the test cake quickly and cool it to room temperature with a fan to obtain phosphate aluminate cement clinker. The XRD analysis diagram of the clinker is as follows Figure 1 The quantitative results of clinker minerals are shown in Table 3.
[0028] Example 2
[0029] The production method of high-gelling aluminophosphate cement using a low-quality raw material in Example 2 is as follows: The low-grade limestone, phosphate tailings, etc. are crushed, and the raw materials are ground by planetary mill to a fineness of 74μm square hole sieve with a sieve residue of <5%. Raw material ratio: limestone 15.69%, phosphate tailings 40.29%, aluminum ash 44.02%, and the ingredients are mixed by a measuring scale. The chemical composition of each raw material is shown in Table 1. 1% CaF2 is added to the weighed raw materials and mixed to prepare raw material powder. Add 5% water by weight to the raw material powder, mix evenly, press it into a test cake of Ф×8mm (thickness) with a press, and dry it in a dryer at 105℃. The test cake is placed in a high-temperature furnace for calcination, and the heating rate is 10℃ / min. After the temperature reaches 950℃, keep it warm for half an hour, and then heat it to 1530℃ and keep it warm for 2 hours. Take out the test cake quickly and cool it to room temperature with a fan to obtain phosphate aluminate cement clinker. The XRD analysis diagram of the clinker is as follows Figure 1 The quantitative results of clinker minerals are shown in Table 3.
[0030] Example 3
[0031] The production method of high-gelling aluminophosphate cement using a low-quality raw material in Example 3 is as follows: The low-grade limestone, phosphate tailings, etc. are crushed, and the raw materials are ground by planetary mill to a fineness of 74μm square hole sieve with a sieve residue of <5%. Raw material ratio: limestone 17.47%, phosphate tailings 42.85%, aluminum ash 39.68%, and the ingredients are mixed by a measuring scale. The chemical composition of each raw material is shown in Table 1. 1% CaF2 is added to the weighed raw materials and mixed to prepare raw material powder. Add 5% water by weight to the raw material powder, mix evenly, press it into a test cake of Ф×8mm (thickness) with a press, and dry it in a dryer at 105℃. The test cake is placed in a high-temperature furnace for calcination, with a heating rate of 10℃ / min. After the temperature reaches 950℃, keep it warm for half an hour, and then heat it to 1530℃ and keep it warm for 2 hours. Take out the test cake quickly and cool it to room temperature with a fan to obtain phosphate aluminate cement clinker. The XRD analysis diagram of the clinker is as follows Figure 1 The quantitative results of clinker minerals are shown in Table 3.
[0032] Example 4
[0033] The production method of high-gelling aluminophosphate cement using a low-quality raw material in Example 4 is as follows: The low-grade limestone, phosphate tailings, etc. are crushed, and the raw materials are ground by planetary mill to a fineness of 74μm square hole sieve with a sieve residue of <5%. Raw material ratio: 18.85% limestone, 38.4% phosphate tailings, 42.75% aluminum ash, and the ingredients are mixed by a measuring scale. The chemical composition of each raw material is shown in Table 1. 1% CaF2 is added to the weighed raw materials and mixed to prepare raw material powder. Add 5% water by weight to the raw material powder, mix evenly, press it into a test cake of Ф×8mm (thickness) with a press, and dry it in a dryer at 105℃. The test cake is placed in a high-temperature furnace for calcination, with a heating rate of 10℃ / min. After the temperature reaches 950℃, keep it warm for half an hour, and then heat it to 1530℃ and keep it warm for 2 hours. Take out the test cake quickly and cool it to room temperature with a fan to obtain phosphate aluminate cement clinker. The XRD analysis diagram of the clinker is as follows Figure 1 The quantitative results of clinker minerals are shown in Table 3.
[0034] Table 3 Clinker mineral composition (wt / %)
[0035] After the above-mentioned phosphate aluminate cement clinker was crushed, it was ground by a planetary mill and mixed with water to make a cement paste product. The setting time and compressive strength of the phosphate aluminate cement samples were tested at 1 day, 3 days and 28 days. The test results are shown in Tables 4 and 5.
[0036] Table 4 Setting time of phosphate-aluminate cement slurry (min)
[0037] Table 5 Compressive strength and carbonation depth of phosphate aluminate cement
[0038] It can be seen from Tables 4 and 5 that the high-gelling phosphate aluminate cement prepared by the present invention using inferior raw materials has high early compressive strength, and the strength continues to increase in the middle and late stages. Compared with other embodiments, Example 4 with more calcium phosphate aluminate phase has higher cement strength. At the same time, phosphate aluminate cement has a lower carbonization depth and better CO2 corrosion resistance.
[0039] Combination Figure 1 From the clinker mineral composition shown in the figure, it can be seen that the higher the CAP and C2S contents in the phosphate aluminate cement prepared from inferior materials, the shorter the setting time, the higher the early and late compressive strength of the cement, and the better the CO2 corrosion resistance. This is mainly because CAP promotes early hydration and performance development, C2S promotes late performance development, and at the same time, the hydration product of phosphate aluminate cement has a low content of calcium hydroxide, so it has good CO2 corrosion resistance.
[0040] The present invention uses low-grade limestone, phosphorus tailings and other inferior materials to prepare high-gelling aluminophosphate cement, which has low production cost and wide selection of raw materials, reduces the pollution of solid waste to the environment, and complies with the carbon reduction policy of the cement industry.
[0041] The present invention provides a method and idea of preparing high-gelling phosphate aluminate cement and method using inferior raw materials. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A method for preparing high-gelling aluminophosphate cement using inferior raw materials, characterized in that: The steps include: (1) Crushing, drying and grinding calcium raw materials, phosphate rock and aluminum raw materials together, and mixing and homogenizing to obtain raw materials; wherein the raw materials have a weight percentage of: 35-40% CaO, 45-60% Al2O3, 5-10% P2O5, 5-10% SiO2, and other impurities of 1-10%; (2) heating the raw material obtained in step (1) to 900-950° C. at a heating rate of 5-10° C. / min, keeping the temperature for 30 min, and then heating the raw material to 1460-1530° C. at a heating rate of 5-10° C. / min, keeping the temperature for 60-120 min, to obtain a calcined clinker block; (3) The calcined clinker block obtained in step (2) is cooled by air cooling and then ground to obtain a calcined clinker block.
2. The method for preparing high gelling aluminophosphate cement using inferior raw materials according to claim 1, characterized in that: The calcium raw material comprises at least one of low-grade limestone, quicklime or slaked lime; wherein the mass percentage of CaO is 40-50%.
3. The method for preparing high gelling aluminophosphate cement using inferior raw materials according to claim 1, characterized in that: The phosphate rock comprises at least one of phosphate rock powder and phosphate ore tailings, and includes the following components in percentage by mass: 20-25% of P2O5, 40-48% of CaO, and 5-10% of SiO2.
4. The method for preparing high gelling aluminophosphate cement using inferior raw materials according to claim 1, characterized in that: The aluminum raw material includes at least one of aluminum ash, coal gangue and fly ash, and includes the following components in percentage by mass: 5-9% MgO, 75-85% Al2O3 and 5-8% SiO2.
5. The method for preparing high gelling aluminophosphate cement using inferior raw materials according to claim 1, characterized in that: In step (1), the calcium raw material, phosphate rock and aluminum raw material are mixed in a mass ratio of (15-25): (35-45): (35-45) to obtain raw material.
6. The method for preparing high gelling aluminophosphate cement using inferior raw materials according to claim 1, characterized in that: In step (1), other impurities in the raw material at least contain MgO and SO3.
7. The method for preparing high gelling aluminophosphate cement using inferior raw materials according to claim 1, characterized in that: In step (1), the raw material is further mixed with 0.5-1.5% by mass of CaF2.
8. The method for preparing high gelling aluminophosphate cement using inferior raw materials according to claim 6, characterized in that: In step (1), the calcium raw material, phosphate rock and aluminum raw material are ground to 200-400 meshes and then fully mixed with CaF2.
9. Aluminophosphate cement prepared by the preparation method according to any one of claims 1 to 8.
10. Aluminophosphate cement according to claim 9, characterized in that: The percentage content of mineral composition is as follows: 45~60% CAP, 15~25% CA2, 10~20% C2AS, 2~10% C2S, 3~15% MA, and 1~10% other mineral phases.