Anti-seismic crack gypsum board and processing method thereof

By optimizing material ratio and processing methods, and using modified glass fiber and polycarboxylic acid water reducing agents, the seismic resistance of gypsum board is improved, and the problem of insufficient seismic resistance of traditional gypsum boards is solved, and higher strength and toughness are achieved , ensure the stability and durability of buildings in disasters such as earthquakes.

CN118955069AInactive Publication Date: 2024-11-15WUJIANG SECOND CONSTR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410924483.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional gypsum boards have poor structural brittleness and crack resistance in terms of seismic resistance, and are prone to cracks and ruptures due to external forces such as earthquakes, affecting the stability and safety of buildings.

Method used

By optimizing material ratio and processing methods, modifying glass fibers and polycarboxylic acid water reducers are used to form a closely-bonded gypsum board structure, improving its strength and toughness and enhancing seismic resistance. Specific methods include the preparation of modified glass fibers and the modification of polyacrylamide binder, combined with a three-stage drying process to improve overall performance.

Benefits of technology

It significantly improves the seismic resistance of gypsum board, can effectively suppress the generation and expansion of cracks, ensure the integrity and stability of gypsum board, and can be moderately deformed when subjected to external forces to absorb and dissipate energy, and reduce the formation of cracks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides an anti-seismic crack gypsum board and a processing method thereof, and relates to the technical field of building materials. The anti-seismic crack gypsum board comprises the following materials in parts by weight: 100-120 parts of gypsum powder; the concrete comprises the following components in parts by weight: 30-40 parts of modified glass fibers, 12-16 parts of sand, 1-3 parts of a binder, 0.5-1 part of a polycarboxylate superplasticizer and 120-140 parts of water. According to the anti-seismic crack gypsum board disclosed by the invention, uniform distribution and tight connection of the internal structure of the gypsum board are realized by elaborately adjusting the proportion of the gypsum powder, the sand, the binder, the polycarboxylate superplasticizer and the like. The optimized proportion not only ensures the strength of the plasterboard, but also improves the toughness and durability of the plasterboard, so that the plasterboard can better maintain integrity when being vibrated, and after the raw material proportion is adjusted, the anti-cracking effect of the plasterboard is enhanced, and meanwhile, the heat storage performance of the plasterboard during use is enhanced; the speed of cold and hot air exchange on the two sides of the gypsum board is reduced, and the energy-saving effect of the gypsum board is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a shatter-resistant gypsum board and a processing method thereof. Background Art

[0002] Gypsum board has become an indispensable material in the construction industry due to its excellent sound insulation and flame retardant properties, clean and environmentally friendly characteristics during the production process, highly automated production processes, and efficient recycling of raw materials. It is widely used in the fields of luxurious decoration of commercial real estate, practical partitions of public buildings, and warm ceilings of family homes, providing beautiful and practical solutions for various types of building spaces. In the current market, paper-faced gypsum board and fiber gypsum board are the two major mainstream products. Among them, paper-faced gypsum board occupies about 80% of the market share with its relatively low cost and wide range of application scenarios.

[0003] In the construction industry, gypsum board is a common lightweight building material that is widely favored for its good thermal insulation, sound insulation and fire resistance. However, when facing natural disasters such as earthquakes, the seismic resistance of traditional gypsum board is often insufficient, and it is easy to crack or even break due to external forces, which seriously affects the stability and safety of the building. Therefore, how to improve the seismic resistance of gypsum board has become an urgent problem to be solved in the current field of building materials.

[0004] The main problem with traditional gypsum boards in terms of seismic performance is their structural brittleness and poor crack resistance. When subjected to external forces such as earthquakes, gypsum boards often lack sufficient strength and toughness to effectively absorb and dissipate energy, leading to the generation and expansion of cracks. In addition, although the adhesive used in traditional gypsum boards has certain bonding properties, the network structure formed inside the gypsum boards is not stable enough, which also affects the overall strength and seismic performance of the gypsum boards.

[0005] In order to overcome the above problems, researchers began to explore ways to improve the seismic performance of gypsum boards by optimizing the material ratio and processing methods. Among them, the introduction of reinforcing materials such as modified glass fibers has become an effective means. Modified glass fibers have excellent mechanical properties and crack resistance, and can significantly improve the strength and toughness of gypsum boards. At the same time, through reasonable material ratios and processing methods, a tight bond can be formed between the modified glass fibers and the gypsum matrix, thereby improving the overall performance of the gypsum board. Based on this, the present invention provides a seismic crack-resistant gypsum board and a processing method thereof. Summary of the invention

[0006] The purpose of the present invention is to provide a shatter-resistant gypsum board and a processing method thereof, which optimizes the mechanical properties and shatter-resistant properties of the shatter-resistant gypsum board.

[0007] On the one hand, the present invention provides a shatter-resistant gypsum board, comprising the following materials in parts by weight: 100-120 parts of gypsum powder; 30-40 parts of modified glass fiber, 12-16 parts of sand, 1-3 parts of binder, 0.5-1 parts of polycarboxylate water reducer, and 120-140 parts of water.

[0008] Furthermore, the preparation method of the modified glass fiber includes: dissolving an aqueous curing agent in water to obtain an aqueous curing agent solution; then adding SiO2 into water and stirring to form a SiO2 suspension, mixing the suspension with the aqueous curing agent solution and stirring, adding an aqueous epoxy resin and stirring to uniformly disperse the nano-SiO2 to obtain a mixed solution; taking the glass fiber and completely immersing it in the mixed solution and letting it stand, taking it out and drying it to obtain the SiO2 modified glass fiber.

[0009] Furthermore, the weight ratio of the water-based curing agent, the total amount of water, SiO2, and the water-based epoxy resin is (2-3): (20-30): (2-4): (2-3).

[0010] Furthermore, the standing time is 50-60 minutes.

[0011] Furthermore, the binder is a modified polyacrylamide binder.

[0012] Furthermore, the preparation method of the modified polyacrylamide binder comprises: mixing 80-90wt% polyacrylamide and 10-20wt% modifier OP-10 and stirring for 30-60 minutes to obtain a uniform interface modified polyacrylamide binder.

[0013] Furthermore, the molecular weight of the polyacrylamide is 3,000,000-5,000,000.

[0014] Furthermore, the polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of (1-2):1.

[0015] On the other hand, the present invention also provides a method for processing shatter-resistant gypsum board, the steps comprising: weighing various required materials, putting the materials into a mixer, and evenly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the shatter-resistant gypsum board after drying.

[0016] Furthermore, the drying is a three-stage drying method, specifically drying at 200-220°C for 10-12 minutes, drying at 160-180°C for 18-20 minutes, and drying at 100-120°C for 40-50 minutes.

[0017] The beneficial effects of the present invention are: The present invention successfully endows the gypsum board with both sufficient strength and excellent flexibility and deformation capacity through a carefully designed material ratio, including the ratio of gypsum powder, modified glass fiber, sand, and the appropriate amount of water and polycarboxylate water reducer; this ratio enables the raw materials such as gypsum powder, modified glass fiber, sand to be tightly combined to form a gypsum board with strong integrity and tight structure. When external forces such as earthquakes act on the gypsum board, the modified glass fiber can effectively inhibit the generation and expansion of cracks, ensuring the integrity and stability of the gypsum board. At the same time, this reasonable ratio enables the gypsum board to deform moderately when encountering external forces such as earthquakes, thereby absorbing and dissipating energy and significantly reducing the formation of cracks.

[0018] The present invention introduces an appropriate amount of SiO2 nanoparticles during the glass fiber modification process, which can significantly improve the seismic resistance of the gypsum board. When the glass fiber is modified with SiO2 nanoparticles, the SiO2 adhesion layer on the surface of the glass fiber begins to appear, so that the SiO2 layer forms a unique "gully" defect structure; this structure helps to absorb and disperse energy through the deformation of the "gully" when impacted by external forces, thereby improving the seismic resistance of the gypsum board; and the water-based epoxy resin has certain film-forming properties, and can also effectively fill the pores at the fiber interface inside the composite material, which not only forms a good interface reinforcement layer on the surface of the glass fiber, but also enhances the bonding force between the glass fiber and the gypsum matrix, thereby improving the overall strength of the gypsum board. The modified glass fiber can significantly improve the stability and durability of the gypsum board in natural disasters such as earthquakes.

[0019] The present invention utilizes the modifier OP-10 to modify polyacrylamide, and the oxygen atoms on the ethoxyl group and the phenolic hydroxyl group in the OP-10 interfacial modifier can form an O---HN type hydrogen bond with the nitrogen atom of the amide group in the polyacrylamide. The formation of this hydrogen bond changes the hydrogen bond network inside the polyacrylamide molecule, and the intramolecular hydrogen bond inside the original polyacrylamide is partially destroyed due to the interaction with OP-10, reducing the crosslinking and entanglement between the polyacrylamide molecular chains, making the polyacrylamide molecular chains more flexible and the fluidity enhanced. Due to the reduction of the crosslinking of the polyacrylamide molecular chains, the dispersibility of polyacrylamide in the gypsum board is improved, and it can be more evenly distributed in the gypsum board to form a more stable network structure. In addition, the addition of OP-10 also enhances the interaction between polyacrylamide and gypsum particles, improves the compatibility between the two, and makes the structure inside the gypsum board more compact and firm. When the gypsum board is subjected to external forces such as earthquakes, the polyacrylamide binder, as an important component inside, the flexibility and fluidity of its molecular chains can effectively dissipate and absorb part of the energy, reducing the concentrated transmission of energy. The hydrogen bond network formed by polyacrylamide and OP-10 can also provide a certain elasticity and deformation capacity, further increasing the energy dissipation capacity of the gypsum board when subjected to force, and improving the overall strength and stability of the gypsum board. This enhanced interface bonding strength makes the gypsum board less likely to be damaged or peeled off when subjected to external forces, thereby improving its seismic performance.

[0020] The present invention uses 2-phenoxyethyl acrylate and polyhexadecanol maleate in the ratio (1-2):1 as a composite water reducer, which has a certain synergistic effect. The synergistic effect comes from the complementarity of the two materials in the molecular structure. The phenoxy group in the 2-phenoxyethyl acrylate has a good plasticizing effect, which can increase the flexibility and ductility of the gypsum board material and improve its processing performance; polyhexadecanol maleate is used as a polycarboxylic acid water reducer, which can improve the workability of concrete without changing the strength of concrete, so that the gypsum board has better flexibility while maintaining sufficient strength.

[0021] The present invention mixes the raw materials and process for preparing the anti-shattering gypsum board, effectively improves the synergistic effect between the raw materials, and optimizes the performance of the anti-shattering gypsum board to the maximum extent. The main raw materials of the anti-shattering gypsum board of the present invention are environmentally friendly materials such as gypsum powder and modified glass fiber, which do not contain harmful substances and meet the national environmental protection standards; at the same time, its production process has low energy consumption and little pollution, which meets the requirements of sustainable development. DETAILED DESCRIPTION

[0022] The technical scheme of the present invention is described clearly and completely below. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. It should be noted that the following raw materials are all commercially available. Example

[0023] The present embodiment provides a shatter-resistant gypsum board, comprising the following materials by weight: 110 parts of gypsum powder; 35 parts of modified glass fiber, 14 parts of sand, 2 parts of modified polyacrylamide binder, 0.7 parts of polycarboxylic acid water reducer, and 130 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2.5g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 30 minutes; then adding 3g of water-based epoxy resin STW600K to the above mixed solution, and stirring for 45 minutes to evenly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is evenly dispersed, and after standing for 55 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0024] The preparation method of the modified polyacrylamide binder comprises: mixing 85wt% polyacrylamide and 15wt% modifier OP-10 and stirring for 45 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 4,000,000.

[0025] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 1.5:1.

[0026] The processing method of the anti-shattering gypsum board in this embodiment comprises the following steps: weighing various required materials, putting the materials into a mixer, and evenly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes. Example

[0027] The present embodiment provides a shatter-resistant gypsum board, comprising the following materials in parts by weight: 100 parts of gypsum powder; 30 parts of modified glass fiber, 12 parts of sand, 1 part of modified polyacrylamide binder, 0.5 parts of polycarboxylic acid water reducer, and 120 parts of water; The preparation method of the modified glass fiber includes: dissolving 2g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 20 minutes; then adding 2g of water-based epoxy resin STW600K to the above mixed solution and stirring for 30 minutes to uniformly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is uniformly dispersed, and after standing for 50 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0028] The preparation method of the modified polyacrylamide binder comprises: mixing 80wt% polyacrylamide and 20wt% modifier OP-10 and stirring for 30 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 3,000,000.

[0029] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 1:1.

[0030] The processing method of the anti-shattering gypsum board in this embodiment comprises the following steps: weighing various required materials, putting the materials into a mixer, and evenly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 200°C for 12 minutes, drying at 160°C for 20 minutes, and drying at 100°C for 50 minutes. Example

[0031] The present embodiment provides a shatter-resistant gypsum board, comprising the following materials by weight: 120 parts of gypsum powder; 40 parts of modified glass fiber, 16 parts of sand, 3 parts of modified polyacrylamide binder, 1 part of polycarboxylic acid water reducer, and 140 parts of water; The preparation method of the modified glass fiber includes: dissolving 3g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 3g of SiO2 and adding 10g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 20 minutes; then adding 4g of water-based epoxy resin STW600K to the mixed solution and stirring for 30 minutes to uniformly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is uniformly dispersed. After standing for 60 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber. At this time, it is taken out and placed in a vacuum drying oven at 60°C for 3 hours to obtain SiO2 modified glass fiber.

[0032] The preparation method of the modified polyacrylamide binder comprises: mixing 90wt% polyacrylamide and 10wt% modifier OP-10, and stirring for 60 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 5,000,000.

[0033] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 2:1.

[0034] The processing method of the anti-shattering gypsum board in this embodiment comprises the following steps: weighing various required materials, putting the materials into a mixer, and evenly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 220°C for 10 minutes, drying at 180°C for 18 minutes, and drying at 120°C for 40 minutes. Example

[0035] The present embodiment provides a shatter-resistant gypsum board, comprising the following materials in parts by weight: 100 parts of gypsum powder; 40 parts of modified glass fiber, 12 parts of sand, 3 parts of modified polyacrylamide binder, 0.5 parts of polycarboxylic acid water reducer, and 140 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2.5g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 30 minutes; then adding 3g of water-based epoxy resin STW600K to the above mixed solution, and stirring for 45 minutes to evenly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is evenly dispersed, and after standing for 55 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0036] The preparation method of the modified polyacrylamide binder comprises: mixing 85wt% polyacrylamide and 15wt% modifier OP-10 and stirring for 45 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 4,000,000.

[0037] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 1.5:1.

[0038] The processing method of the anti-shattering gypsum board in this embodiment comprises the following steps: weighing various required materials, putting the materials into a mixer, and evenly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0039] This comparative example provides a gypsum board, comprising the following materials by weight: 110 parts of gypsum powder; 35 parts of modified glass fiber, 14 parts of sand, 2 parts of modified polyacrylamide binder, 0.7 parts of polycarboxylic acid water reducer, and 130 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2.5g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 30 minutes to uniformly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is uniformly dispersed, and after standing for 55 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0040] The preparation method of the modified polyacrylamide binder comprises: mixing 85wt% polyacrylamide and 15wt% modifier OP-10 and stirring for 45 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 4,000,000.

[0041] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 1.5:1.

[0042] The processing method of the gypsum board in this comparative example comprises the following steps: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0043] This comparative example provides a gypsum board, comprising the following materials by weight: 110 parts of gypsum powder; 35 parts of modified glass fiber, 14 parts of sand, 2 parts of modified polyacrylamide binder, 0.7 parts of polycarboxylic acid water reducer, and 130 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then adding 3g of water-based epoxy resin STW600K to the curing agent aqueous solution, stirring for 45 minutes to uniformly disperse to obtain a mixed solution; then taking the glass fiber and completely immersing it in the mixed solution, standing it for 55 minutes, taking it out and placing it in a vacuum drying oven at 60°C to fully dry it for 3 hours, thereby obtaining the modified glass fiber.

[0044] The preparation method of the modified polyacrylamide binder comprises: mixing 85wt% polyacrylamide and 15wt% modifier OP-10 and stirring for 45 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 4,000,000.

[0045] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 1.5:1.

[0046] The processing method of the gypsum board in this comparative example comprises the following steps: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0047] This comparative example provides a gypsum board, comprising the following materials in parts by weight: 110 parts of gypsum powder; 35 parts of glass fiber, 14 parts of sand, 2 parts of modified polyacrylamide binder, 0.7 parts of polycarboxylic acid water reducer, and 130 parts of water; The preparation method of the modified polyacrylamide binder comprises: mixing 85wt% polyacrylamide and 15wt% modifier OP-10 and stirring for 45 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 4,000,000.

[0048] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 1.5:1.

[0049] The processing method of the gypsum board in this comparative example comprises the following steps: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0050] This comparative example provides a gypsum board, comprising the following materials by weight: 110 parts of gypsum powder; 35 parts of modified glass fiber, 14 parts of sand, 2 parts of polyacrylamide binder, 0.7 parts of polycarboxylic acid water reducer, and 130 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2.5g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 30 minutes; then adding 3g of water-based epoxy resin STW600K to the above mixed solution, and stirring for 45 minutes to evenly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is evenly dispersed, and after standing for 55 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0051] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 1.5:1.

[0052] The processing method of the gypsum board in this comparative example comprises the following steps: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0053] This comparative example provides a gypsum board, comprising the following materials in parts by weight: 110 parts of gypsum powder; 35 parts of modified glass fiber, 14 parts of sand, 0.7 parts of polycarboxylate water reducer, and 130 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2.5g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 30 minutes; then adding 3g of water-based epoxy resin STW600K to the above mixed solution, and stirring for 45 minutes to evenly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is evenly dispersed, and after standing for 55 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0054] The polycarboxylic acid water-reducing agent comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of 1.5:1.

[0055] The processing method of the gypsum board in this comparative example comprises the following steps: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0056] This comparative example provides a gypsum board, comprising the following materials by weight: 110 parts of gypsum powder; 35 parts of modified glass fiber, 14 parts of sand, 2 parts of modified polyacrylamide binder, 0.7 parts of polycarboxylic acid water reducer, and 130 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2.5g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 30 minutes; then adding 3g of water-based epoxy resin STW600K to the above mixed solution, and stirring for 45 minutes to evenly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is evenly dispersed, and after standing for 55 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0057] The preparation method of the modified polyacrylamide binder comprises: mixing 85wt% polyacrylamide and 15wt% modifier OP-10 and stirring for 45 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 4,000,000.

[0058] The polycarboxylate water reducer is 2-phenoxyethyl acrylate.

[0059] The processing method of the gypsum board in this comparative example comprises the following steps: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0060] This comparative example provides a gypsum board, comprising the following materials by weight: 110 parts of gypsum powder; 35 parts of modified glass fiber, 14 parts of sand, 2 parts of modified polyacrylamide binder, 0.7 parts of polycarboxylic acid water reducer, and 130 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2.5g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 30 minutes; then adding 3g of water-based epoxy resin STW600K to the above mixed solution, and stirring for 45 minutes to evenly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is evenly dispersed, and after standing for 55 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0061] The preparation method of the modified polyacrylamide binder comprises: mixing 85wt% polyacrylamide and 15wt% modifier OP-10 and stirring for 45 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 4,000,000.

[0062] The polycarboxylate water reducer is polyhexadecanol maleate.

[0063] The processing method of the gypsum board in this comparative example comprises the following steps: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0064] This comparative example provides a gypsum board, comprising the following materials by weight: 110 parts of gypsum powder; 35 parts of modified glass fiber, 14 parts of sand, 2 parts of modified polyacrylamide binder, and 130 parts of water; The preparation method of the modified glass fiber includes: dissolving 2.5g of water-based curing agent BAYHYDUR XP 2655 in 15g of water to obtain a curing agent aqueous solution; then taking 2.5g of SiO2 and adding 5g of deionized water, stirring for 10 minutes to form a SiO2 suspension, and adding the suspension to the curing agent aqueous solution and stirring for 30 minutes; then adding 3g of water-based epoxy resin STW600K to the above mixed solution, and stirring for 45 minutes to evenly disperse the nano-SiO2; then taking the glass fiber and completely immersing it in the mixed solution after the nano-SiO2 is evenly dispersed, and after standing for 55 minutes, the nano-SiO2 will be deposited on the surface of the glass fiber, and then taking it out and placing it in a vacuum drying oven at 60°C to fully dry for 3 hours to obtain SiO2 modified glass fiber.

[0065] The preparation method of the modified polyacrylamide binder comprises: mixing 85wt% polyacrylamide and 15wt% modifier OP-10 and stirring for 45 minutes to obtain a uniform interface modified polyacrylamide binder; the molecular weight of the polyacrylamide is 4,000,000.

[0066] The processing method of the gypsum board in this comparative example comprises the following steps: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shattering gypsum board after drying; wherein the drying is a three-stage drying method, specifically drying at 210°C for 11 minutes, drying at 170°C for 19 minutes, and drying at 110°C for 45 minutes.

[0067] Test Example 1: The gypsum board slurry prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-8 was flowed from a mixer onto the pre-laid lower face paper, and the upper face paper was supplied at the same time, and formed into a board by roller pressing. The formed board was dried, coagulated and hardened, and then cut after hardening to prepare a 9.5 mm ordinary paper-faced gypsum board. The performance was then explored, and the performance test results are shown in Table 1 below: Table 1 Finally, it should be noted that the above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. All technical solutions and improvements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A shatter-resistant gypsum board, characterized in that: Contains the following materials by weight: 100-120 parts of gypsum powder; 30-40 parts of modified glass fiber, 12-16 parts of sand, 1-3 parts of binder, 0.5-1 parts of polycarboxylate water reducer, 120-140 parts of water; The binder is a modified polyacrylamide binder; the preparation method of the modified polyacrylamide binder comprises: mixing 80-90wt% polyacrylamide and 10-20wt% modifier OP-10, and stirring for 30-60 minutes to obtain a uniform interface modified polyacrylamide binder.

2. The anti-shattering gypsum board according to claim 1, characterized in that: The preparation method of the modified glass fiber comprises: dissolving an aqueous curing agent in water to obtain a curing agent aqueous solution; adding SiO2 into the water and stirring to form a SiO2 suspension, mixing the suspension with the curing agent aqueous solution and stirring, adding an aqueous epoxy resin and stirring to uniformly disperse the nano-SiO2 to obtain a mixed solution; taking a glass fiber and completely immersing it in the mixed solution and letting it stand, taking it out and drying it to obtain the SiO2 modified glass fiber.

3. The anti-shattering gypsum board according to claim 2, characterized in that: The weight ratio of the water-based curing agent, the total amount of water, SiO2, and the water-based epoxy resin is (2-3): (20-30): (2-4): (2-3).

4. The anti-shatter gypsum board according to claim 1, characterized in that: The standing time is 50-60 min.

5. The anti-shattering gypsum board according to claim 1, characterized in that: The molecular weight of the polyacrylamide is 3,000,000-5,000,000.

6. The anti-shattering gypsum board according to claim 1, characterized in that: The polycarboxylic acid water reducer comprises 2-phenoxyethyl acrylate and polyhexadecanol maleate in a weight ratio of (1-2):

1.

7. A method for processing a shatter-resistant gypsum board according to any one of claims 1 to 6, characterized in that: The steps include: weighing various required materials, putting the materials into a mixer, and uniformly mixing them to obtain slurry; pouring and paving the slurry in a mold, and obtaining the anti-shaking gypsum board after drying.

8. The processing method according to claim 7, characterized in that: The drying is a three-stage drying method, which is drying at 200-220° C. for 10-12 minutes, drying at 160-180° C. for 18-20 minutes, and drying at 100-120° C. for 40-50 minutes.