Indium titanium tantalum cerium oxide target material and preparation method and application thereof

By doping similar metal elements into the indium cerium tantalum titanium target and adopting a two-step sintering method, the problem of insufficient target density and mobility in the prior art is solved, and the high density of indium titanium tantalum cerium target is achieved. and conductivity meet the requirements of high transmittance and low resistivity.

CN118955091AActive Publication Date: 2024-11-15XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD

Patent Information

Application Number
CN202410880988.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The existing indium titanium tantalum cerium target process is difficult to significantly improve the density and mobility of the target, resulting in its performance not enough to meet the requirements of high permeability and low resistivity.

Method used

By doping metal elements with similar ion radius to the indium cerium tantalum titanium target, and using a two-step sintering method, large pores are eliminated at the highest temperature and insulation at low temperatures to eliminate small-size unstable pores, improving density and electrical conductivity sex.

Benefits of technology

The density and mobility of indium titanium tantalum cerium targets are significantly improved, the resistivity is reduced, its density and conductivity are improved, and the requirements of high transmissivity and low resistivity are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004924499180000081
    Figure BDA0004924499180000081
  • Figure BDA0004924499180000091
    Figure BDA0004924499180000091
Patent Text Reader

Abstract

The invention belongs to the field of solar targets, and discloses a preparation method of an indium titanium tantalum cerium oxide target, which comprises the following steps: mixing a metal oxide, an auxiliary agent and deionized water, pulping, ball-milling and sieving to obtain powder I; drying, crushing and sieving the obtained powder I to obtain powder II; carrying out mould pressing and cold isostatic pressing on the obtained powder II to obtain a target precursor; finally, the obtained target material precursor is placed in a sintering furnace to be sintered and cooled to the room temperature, and the indium titanium tantalum cerium oxide target material is obtained.In addition, the indium titanium tantalum cerium oxide target material is further disclosed, the indium titanium tantalum cerium oxide target material is obtained by doping tin elements with similar ion radiuses into the indium cerium tantalum titanium oxide target material and adopting a two-step sintering process, and the indium titanium tantalum cerium oxide target material is obtained. The density and the electron mobility of the target material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar energy target materials, and in particular to an indium titanium tantalum cerium oxide target material and a preparation method and application thereof. Background Art

[0002] Transparent conductive oxide thin film TCO thin film is a thin film material with high transmittance and low resistivity in the visible light spectral range of 380nm to 780nm. It has good metal-like conductivity, glass-like high light transmittance, high reflectivity in the infrared region and other excellent semiconductor properties. It is widely used in displays, solar cells, light-emitting diodes, touch screens, gas sensors, as well as microelectronics, vacuum electronic devices and other fields. In the field of solar cells, when light is incident from the top cell to the surface of the middle connecting layer TCO, light reflection and transmission will occur: in the stacked solar cell, the top cell needs to absorb ultraviolet-visible light 300 to 780nm and the near-infrared light (780 to 1400nm) is absorbed and utilized by the bottom cell. Therefore, the middle TCO layer is required to have the following characteristics: (1) Good optical transmittance: its transmittance in the visible light band of 380nm to 780nm is greater than 80%; (2) Good conductivity: its resistivity is generally less than 10 -3 Ω.cm; (3) Wide band gap.

[0003] There are many types of TCO films, the most common of which are films doped with neighboring cations or anions based on zinc oxide-based ZnO, tin oxide-based SnO2, indium oxide-based In2O3, etc. Since tin replaces indium, this target material increases the mobility of impurity ions, thereby increasing the carrier mobility and reducing the resistivity of the target material, making tin doping a hot topic of research.

[0004] Among them, Chinese patent application 202310691428.4 discloses an indium oxide titanium tantalum cerium target material obtained based on a high-temperature sintering method and a preparation method thereof. The preparation method is: indium oxide, titanium oxide, tantalum oxide, cerium oxide, dispersant, binder, and deionized water are mixed to make a slurry and ball milled; the slurry after ball milling is dried and calcined to obtain a powder; the powder is subjected to hydraulic forming and cold isostatic pressing to obtain an indium oxide cerium tantalum titanium precursor; and the indium oxide cerium tantalum titanium precursor is subjected to high-temperature sintering to obtain an indium oxide cerium tantalum titanium target material.

[0005] This scheme utilizes indium oxide, titanium oxide, tantalum oxide, and cerium oxide for further high-temperature sintering to obtain indium oxide, cerium, tantalum, and titanium targets, thereby improving the relative density and mobility of the targets.

[0006] Chinese patent application 202410193760.2 discloses a high-density and high-mobility indium oxide doped target material and a preparation method thereof. The preparation method is: indium oxide, tin oxide, rare earth oxide, binder, dispersant and stabilizer are mixed and ground, and spray granulation, molding and cold isostatic pressing are performed in sequence to obtain a blank, and then the blank is sintered at high temperature to obtain a high-density and high-mobility indium oxide doped target material.

[0007] This scheme obtains an indium oxide-doped tin target by doping with tin oxide and keeping it at a maximum temperature of 1500-1600°C during the sintering process, thereby improving the density and mobility of the target.

[0008] It is not difficult to see from the above two schemes that the density and mobility of the target material can be improved by sintering with a combination of multiple metal oxides, or doping with tin oxide, and keeping it warm at the highest sintering temperature.

[0009] The problem that this solution needs to solve: How to propose a method to improve the target material process and thus enhance the target material performance. Summary of the invention

[0010] The purpose of the present invention is to provide a method for preparing an indium titanium tantalum cerium oxide target material, by doping the indium titanium tantalum cerium oxide target material with metal elements having similar ion radii and utilizing a two-step sintering method during the sintering process, so that the density and mobility of the obtained indium titanium tantalum cerium oxide target material are significantly improved.

[0011] To achieve the above objectives, the present application discloses a method for preparing an indium titanium tantalum cerium oxide target, comprising the following steps:

[0012] Step 1: Mix the metal oxide, additives and deionized water, perform slurry ball milling, and sieve to obtain powder 1;

[0013] Step 2: drying, crushing and sieving the powder 1 obtained in step 1 to obtain powder 2;

[0014] Step 3: The powder obtained in step 2 is molded and cold isostatically pressed to obtain a target material precursor;

[0015] Step 4: placing the target precursor obtained in step 3 in a sintering furnace, sintering, and cooling to obtain an indium titanium tantalum cerium oxide target;

[0016] The metal oxide in step 1 is indium oxide, titanium oxide, tantalum oxide, or cerium oxide;

[0017] The sintering process in step 4 is: in the presence of oxygen, heat up to 400-900°C at 0.05-0.5°C / min, and keep warm for 3-6 hours; then heat up to 1350-1500°C at 0.5-1°C / min, and then cool down to 1200-1350°C at 1-3°C / min, and keep warm for 15-30 hours.

[0018] Preferably, step 1 further comprises a dopant, and the dopant is selected from one or more of tin oxide, cadmium oxide, and antimony trioxide.

[0019] Preferably, the mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide and dopant is 97.5-99.5: 0.02-0.2: 0.05-0.5: 0.1-1: 0.01-0.1.

[0020] Preferably, the auxiliary agents in step 1 are dispersants and binders, the dispersant is selected from one or more of polyvinyl pyrrolidone, polycarboxylic acid compounds, and polyvinyl salts; the binder is selected from one or more of polyvinyl alcohol, carboxymethyl cellulose, polyacrylamide, polyacrylic acid salts, and polyethylene glycol.

[0021] Preferably, the mass of the dispersant is 1% to 3% of the total mass of the metal oxide and the dopant; the mass of the binder is 1% to 3% of the total mass of the metal oxide and the dopant; the mass of the deionized water is 30% to 40% of the total mass of the metal oxide and the dopant.

[0022] Preferably, in step 1, the D10 particle size of the powder 1 is 0.05-0.1 um, the D50 particle size is 0.1-0.5 um, and the D90 particle size is 0.5-1 um.

[0023] Preferably, in step 2, a sieve of 60 to 80 mesh is used for sieving.

[0024] Preferably, in step 3, the molding pressure is 30-60 MPa; and the cold isostatic pressing pressure is 350-450 MPa.

[0025] In addition, it also includes an indium titanium tantalum cerium oxide target material, which is prepared by a method for preparing an indium titanium tantalum cerium oxide target material.

[0026] The beneficial effects of the present invention are:

[0027] The invention provides a method for preparing an indium titanium tantalum cerium oxide target material. The indium titanium tantalum cerium oxide target material is doped with a metal element with a similar ion radius, so that the lattice structure of indium oxide shrinks and plays a role as a sintering aid, thereby greatly increasing the compactness and conductivity of the indium titanium tantalum tin-doped indium oxide cerium titanium tantalum target material. A two-step sintering method is used during the sintering process, so that the target material eliminates large pores at a critical density at the highest temperature, and then is kept warm at 50-200°C below the highest temperature. Residual small-sized unstable pores are gradually discharged along with the densification of the target material during the T2 stage of heat preservation, thereby reducing the rate of grain growth and slowly eliminating pores in the blank, thereby achieving a higher density. DETAILED DESCRIPTION

[0028] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0029] Example 1

[0030] Step 1: Indium oxide, titanium oxide, tantalum oxide, cerium oxide, and tin oxide are mixed with polyacrylate, polyvinyl alcohol, and deionized water in a mass ratio of 98.8:0.1:0.45:0.6:0.05, and the mixture is slurried and ball-milled, and sieved to obtain a powder with D10=0.075um, D50=0.3um, and D90=0.75um;

[0031] Step 2: drying the powder 1 obtained in step 1 at 100° C., crushing, and sieving through an 80-mesh sieve to obtain powder 2;

[0032] Step 3: The powder obtained in step 2 is molded at 45 MPa and cold isostatically pressed at 400 MPa to obtain a target material precursor;

[0033] Step 4: placing the target precursor obtained in step 3 in a sintering furnace, heating it to 600°C at 0.3°C / min in the presence of oxygen, and keeping it warm for 4.5 hours; then heating it to 1400°C at 0.7°C / min, and then cooling it to 1300°C at 2°C / min, keeping it warm for 23 hours, and then cooling it to room temperature to obtain an indium titanium tantalum cerium oxide target;

[0034] Example 2

[0035] The method is basically the same as Example 1, except that in step 1, the mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide and tin oxide is 97.5:0.1:0.45:0.6:0.1.

[0036] Example 3

[0037] The method is basically the same as Example 1, except that in step 1, the mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide and tin oxide is 99.5:0.1:0.45:0.6:0.01.

[0038] Example 4

[0039] The method is basically the same as Example 1, except that in step 1, the mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide and cadmium oxide is 98.8:0.1:0.45:0.6:0.05.

[0040] Example 5

[0041] The method is basically the same as Example 1, except that in step 1, the mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide and antimony trioxide is 98.8:0.1:0.45:0.6:0.05.

[0042] Example 6

[0043] It is basically the same as Example 1, except that:

[0044] Step 4: placing the target precursor obtained in step 3 in a sintering furnace, heating it to 400°C at 0.05°C / min in the presence of oxygen, and keeping it warm for 3 hours; then heating it to 1350°C at 0.5°C / min, and then cooling it to 1200°C at 1°C / min, keeping it warm for 15 hours, and then cooling it to room temperature to obtain an indium titanium tantalum cerium oxide target;

[0045] Example 7

[0046] It is basically the same as Example 1, except that:

[0047] Step 4: placing the target precursor obtained in step 3 in a sintering furnace, heating it to 900°C at 0.5°C / min in the presence of oxygen, and keeping it warm for 6 hours; then heating it to 1500°C at 1°C / min, and then cooling it to 1350°C at 3°C / min, keeping it warm for 30 hours, and then cooling it to room temperature to obtain an indium titanium tantalum cerium oxide target;

[0048] Example 8

[0049] It is basically the same as Example 1, except that in step 1, the powder has D10=0.05um, D50=0.1um, and D90=0.5um.

[0050] Example 9

[0051] It is basically the same as Example 1, except that in step 1, the powder has D10=0.1um, D50=0.5um, and D90=1um.

[0052] Comparative Example 1

[0053] The method is basically the same as Example 1, except that in step 1, the mass ratio of indium oxide, titanium oxide, tantalum oxide and cerium oxide is 97.5:0.1:0.45:0.6.

[0054] Comparative Example 2

[0055] It is basically the same as Example 1, except that:

[0056] Step 4: Place the target precursor obtained in step 3 in a sintering furnace, and in the presence of oxygen, heat it to 600°C at 0.3°C / min, and keep it warm for 4.5 hours; then heat it to 1400°C at 0.7°C / min, keep it warm for 23 hours, and cool it to room temperature to obtain an indium titanium tantalum cerium oxide target.

[0057] Comparative Example 3

[0058] It is basically the same as Example 1, except that:

[0059] Step 4: Place the target precursor obtained in step 3 in a sintering furnace, and in the presence of oxygen, heat it to 600°C at 0.3°C / min, and keep it warm for 4.5 hours; then heat it to 1300°C at 0.7°C / min, keep it warm for 23 hours, and cool it to room temperature to obtain an indium titanium tantalum cerium oxide target.

[0060] Comparative Example 4

[0061] It is basically the same as Example 1, except that:

[0062] Step 1: Indium oxide, titanium oxide, tantalum oxide, cerium oxide, and tin oxide are mixed with polyvinyl salt, polyvinyl alcohol, and deionized water in a mass ratio of 98.8:0.1:0.45:0.6:0.05, and the mixture is slurried and ball-milled, and sieved to obtain a powder.

[0063] Performance Testing

[0064] Density detection: The density of the target material is measured by the Archimedes drainage method;

[0065] Mobility: Tested by Hall effect method;

[0066] The performance test results are shown in Table 1:

[0067] Table 1

[0068] Group Relative density% Resistivity uΩ.cm <![CDATA[Mobility cm 2 / V·s]]> Example 1 99.5 327.902 105 Example 2 99.3 373.47 104 Example 3 99.4 376.124 102 Example 4 97.7 676.709 92 Example 5 98.1 688.982 91 Example 6 99.2 382.022 99 Example 7 99.2 384.634 101 Example 8 98.6 581.056 95 Example 9 98.2 635.854 93 Comparative Example 1 97.6 854.264 74 Comparative Example 2 95.8 1065.475 79 Comparative Example 3 97.6 754.254 82 Comparative Example 4 96.5 952.465 89

[0069] Results Analysis

[0070] 1. It can be seen from Example 1 and Comparative Example 1 that when tin oxide is used for doping, the relative density of the prepared indium titanium tantalum cerium oxide target material increases from 97.6% to 99.5%, and the mobility increases from 74 cm 2 / V·s rises to 105cm 2 / V·s, the resistivity dropped from 854.264uΩ.cm to 327.902uΩ.cm, which greatly improved the performance of indium titanium tantalum cerium oxide target. And it can be seen from Table 2:

[0071] Table 2

[0072] Group Relative density% Resistivity uΩ.cm <![CDATA[Mobility cm 2 / V·s]]> Example 1 99.5 327.902 105 Example 2 99.3 373.47 104 Example 3 99.4 376.124 102 Comparative Example 1 97.6 854.264 74

[0073] In Example 1, the mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide, and tin oxide is 98.8:0.1:0.45:0.6:0.05;

[0074] In Example 2, the mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide, and tin oxide is 97.5:0.1:0.45:0.6:0.1;

[0075] In Example 3, the mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide, and tin oxide is 99.5:0.1:0.45:0.6:0.01;

[0076] From the above, it can be seen that when the mass ratio of indium oxide to tin oxide is 97.5-99.5:0.01-0.1, the performance of indium oxide titanium tantalum cerium target is greatly improved.

[0077] 2. It can be seen from Examples 1 and 4-5 that cadmium oxide and antimony trioxide are used to replace tin oxide in Examples 4 and 5, respectively. It can be seen from Table 3 that:

[0078] Table 3

[0079]

[0080]

[0081] When using metal oxides of tin, cadmium and antimony, which are adjacent elements to indium oxide, for doping, the doping of tin oxide has a better effect on improving the performance of indium titanium tantalum cerium oxide target.

[0082] 3. It can be seen from Example 1 and Comparative Examples 2-3 that in Example 1, the sintering process of step 4 is as follows: in the presence of oxygen, the temperature is raised to 600°C at 0.3°C / min and kept at this temperature for 4.5 hours; then the temperature is raised to 1400°C at 0.7°C / min, and then the temperature is lowered to 1300°C at 2°C / min, kept at this temperature for 23 hours, and then lowered to room temperature;

[0083] In comparative example 2, the sintering process of step 4 is as follows: in the presence of oxygen, the temperature is raised to 600° C. at 0.3° C. / min, and kept at that temperature for 4.5 hours; the temperature is then raised to 1400° C. at 0.7° C. / min, and kept at that temperature for 23 hours, and then cooled to room temperature;

[0084] In comparative example 3, the sintering process of step 4 is as follows: in the presence of oxygen, the temperature is raised to 600°C at 0.3°C / min, and kept at that temperature for 4.5 hours; the temperature is then raised to 1300°C at 0.7°C / min, and kept at that temperature for 23 hours, and then cooled to room temperature;

[0085] The properties of the indium titanium tantalum cerium oxide target prepared by the above process are shown in Table 4:

[0086] Table 4

[0087] Group Relative density% Resistivity uΩ.cm <![CDATA[Mobility cm 2 / V·s]]> Example 1 99.5 327.902 105 Comparative Example 2 95.8 1065.475 79 Comparative Example 3 97.6 754.254 82

[0088] It can be seen that the performance of the indium titanium tantalum cerium oxide target materials prepared in Comparative Examples 2 and 3 is much lower than that of the indium titanium tantalum cerium oxide target material prepared in Example 1.

[0089] 4. It can be seen from Example 1, Examples 8-9 and Comparative Example 4 that in Example 1, the particle size of the powder in step 1 is D10 = 0.075um, D50 = 0.3um, and D90 = 0.75um;

[0090] In Example 8, the particle sizes of the powder 1 in step 1 are D10=0.05um, D50=0.1um, and D90=0.5um;

[0091] In Example 9, the particle sizes of the powder 1 in step 1 are D10=0.1um, D50=0.5um, and D90=1um;

[0092] In comparative example 4, step 1 was not screened, and the powder 1 contained particles with a particle size greater than 1 um or less than 0.05 um. The properties of the indium titanium tantalum cerium oxide target prepared by the above process are shown in Table 5:

[0093] Table 5

[0094] Group Relative density% Resistivity uΩ.cm <![CDATA[Mobility cm 2 / V·s]]> Example 1 99.5 327.902 105 Example 8 98.6 581.056 95 Example 9 98.2 635.854 93 Comparative Example 4 96.5 952.465 89

[0095] It can be seen that when the particle size range of powder 1 is controlled within the range of D10 particle size of 0.05-0.1um, D50 particle size of 0.1-0.5um, and D90 particle size of 0.5-1um, the performance of indium titanium tantalum cerium oxide target is better improved.

[0096] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an indium titanium tantalum cerium oxide target, characterized in that: The following steps are included: Step 1: Mix the metal oxide, additives and deionized water, perform slurry ball milling, and sieve to obtain powder 1; Step 2: drying, crushing and sieving the powder 1 obtained in step 1 to obtain powder 2; Step 3: The powder obtained in step 2 is molded and cold isostatically pressed to obtain a target material precursor; Step 4: placing the target material precursor obtained in step 3 in a sintering furnace for sintering and cooling to obtain an indium titanium tantalum cerium oxide target material; The metal oxide in step 1 is indium oxide, titanium oxide, tantalum oxide or cerium oxide; The sintering process in step 4 is: in the presence of oxygen, heating to 400-900°C at 0.05-0.5°C / min, and keeping warm for 3-6 hours; then heating to 1350-1500°C at 0.5-1°C / min, and then cooling to 1200-1350°C at 1-3°C / min, and keeping warm for 15-30 hours.

2. The method for preparing an indium titanium tantalum cerium oxide target according to claim 1, characterized in that: The step 1 further comprises a dopant, and the dopant is selected from tin oxide, cadmium oxide, and antimony trioxide.

3. The method for preparing an indium titanium tantalum cerium oxide target according to claim 1, characterized in that: The mass ratio of indium oxide, titanium oxide, tantalum oxide, cerium oxide and dopant is 97.5-99.5: 0.02-0.2: 0.05-0.5: 0.1-1: 0.01-0.

1.

4. The method for preparing an indium titanium tantalum cerium oxide target according to claim 1, characterized in that: The auxiliary agent in step 1 is a dispersant and a binder, and the dispersant is selected from one or more of polyvinyl pyrrolidone, polycarboxylic acid compounds, and polyvinyl salts; The binder is selected from one or more of polyvinyl alcohol, carboxymethyl cellulose, polyacrylamide, polyacrylic acid salt, and polyethylene glycol.

5. The method for preparing an indium titanium tantalum cerium oxide target according to claim 4, characterized in that: The mass of the dispersant is 1% to 3% of the total mass of the metal oxide and the dopant; the mass of the binder is 1% to 3% of the total mass of the metal oxide and the dopant; the mass of the deionized water is 30% to 40% of the total mass of the metal oxide and the dopant.

6. The method for preparing an indium titanium tantalum cerium oxide target according to claim 1, characterized in that: In the step 1, the D10 particle size of the powder 1 is 0.05-0.1 um, the D50 particle size is 0.1-0.5 um, and the D90 particle size is 0.5-1 um.

7. The method for preparing an indium titanium tantalum cerium oxide target according to claim 1, characterized in that: In step 2, a sieve of 60 to 80 mesh is used for sieving.

8. The method for preparing an indium titanium tantalum cerium oxide target according to claim 1, characterized in that: In step 3, the molding pressure is 30-60 MPa; the cold isostatic pressing pressure is 350-450 MPa.

9. An indium titanium tantalum cerium oxide target, characterized in that: The target is prepared by the method for preparing the indium titanium tantalum cerium oxide target material described in any one of claims 1-8.

Citation Information

Patent Citations

  • Praseodymium-doped indium zinc oxide sputtering target material and preparation method thereof

    CN115925410A

  • Titanium-tantalum-cerium indium oxide target material obtained based on high-temperature sintering method and preparation method of titanium-tantalum-cerium indium oxide target material

    CN116874282A

  • Preparation method of high-density indium oxide doped cerium-titanium-tantalum target material

    CN117185779A

  • Ceramic target material as well as preparation method and application thereof

    CN117486584A

  • High-density and low-resistivity target material for solar energy industry

    CN118184312A

Cited By

  • Method for preparing cerium indium oxide powder based on electrochemical method, cerium indium oxide powder, target material and application of cerium indium oxide powder and target material

    CN119637931A

  • Cerium oxide doped indium oxide-based target material as well as preparation method and application thereof

    CN121135372A