Slurry for preparing compact tantalum carbide coating and sintering method
By using slurry sintering method of tantalum carbide powder, the inefficiency and reliability problems of the chemical vapor deposition method are solved, and high-quality and low-cost dense tantalum carbide coating preparation is achieved, ensuring the coating Stability and high temperature performance.
Patent Information
- Application Number
- CN202410878072.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-02
AI Technical Summary
When the existing tantalum carbide coating is prepared by chemical vapor deposition, the coating has a low deposition rate, long period, high cost and is prone to cracks and pores, resulting in low application reliability and inability to effectively protect the crystals.
The slurry sintering method is adopted with tantalum carbide powder as the main raw material. By mixing volatile organic solvents, tantalum carbide solid powder and sintering aids, forming a suspension for ball milling. After spraying, the temperature and environment are controlled during drying and sintering, and preparation is carried out. Densified tantalum carbide coating.
It has achieved low cost, simple process, short preparation cycle, and prepared a tantalum carbide coating with good suspension stability and good fluidity. The coating has high film formation quality and is firmly combined with the graphite matrix at high temperature to avoid cracks and rises. The skin phenomenon significantly improves the density and bond strength of the coating.
Smart Images

Figure CN118955140A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high temperature resistant and corrosion resistant ceramic coatings, in particular to a slurry and a sintering method for preparing a dense tantalum carbide coating. Background Art
[0002] Tantalum carbide ceramics have a melting point of up to 3880°C, and have high hardness, high thermal conductivity, high bending strength, and low thermal expansion coefficient. They also exhibit excellent thermochemical stability and excellent physical properties, and have good chemical and mechanical compatibility with graphite and C / C composites. Therefore, tantalum carbide coatings are widely used in aerospace thermal protection, single crystal growth, energy electronics, and medical devices. Tantalum carbide coated graphite has better chemical corrosion resistance than bare graphite or SiC coated graphite, can be used stably at high temperatures of 2600°C, and does not react with many metal elements. It is the best coating in the third-generation semiconductor single crystal growth and wafer etching scenarios, and can significantly improve the control of temperature and impurities during the process, and prepare high-quality silicon carbide wafers and related epitaxial wafers. It is especially suitable for the growth of GaN or AlN single crystals by MOCVD equipment and the growth of SiC single crystals by PVT equipment, and the quality of the grown single crystals is significantly improved.
[0003] At present, the chemical vapor deposition (CVD) method is commonly used to prepare tantalum carbide coatings. Its disadvantages are: low coating deposition rate, long deposition cycle, high equipment cost, and the coating is prone to cracks and pores. This fatal defect leads to low reliability in its application, thereby losing its protective effect on the crystal. Summary of the invention
[0004] The present application is made in view of the above-mentioned problems, and its purpose is to provide a method for overcoming the shortcomings of CVD method for preparing tantalum carbide coating, and directly using slurry sintering method with tantalum carbide powder as main raw material to prepare a layer of tantalum carbide coating on a substrate such as graphite; and the slurry sintering method for preparing tantalum carbide coating has significant advantages such as low cost, simple process operation, and short preparation cycle.
[0005] The present application aims to solve the problem of slurry preparation and sintering process for preparing tantalum carbide coating to a certain extent.
[0006] The slurry preparation method for preparing a dense tantalum carbide coating proposed in the present application has simple and easy-to-obtain raw materials, and the prepared slurry has good suspension stability, good fluidity, and is easy to spray, and the coating has high film quality.
[0007] To achieve the above object, the present invention provides a slurry and a sintering method for preparing a dense tantalum carbide coating.
[0008] The first aspect of the present application provides a slurry for preparing a dense tantalum carbide coating, comprising a volatile mixed organic solvent, tantalum carbide solid powder particles insoluble in the solvent, a sintering aid solid powder particles insoluble in the solvent, and a binder soluble in the solvent, which are mixed according to a certain mass fraction. The mixed suspension of the mixed raw material components is ball milled to form a uniformly mixed suspension.
[0009] In any embodiment, the mixed organic solvent is a volatile mixed organic solvent, which is an alcohol or ketone solvent and has good wettability to tantalum carbide solid powder particles and can be suspended in the organic solvent for a long time without sedimentation.
[0010] In any embodiment, the mixed organic solvent is at least two of alcohol and ketone organic solvents such as ethanol, cyclohexanol, glycerol, acetone, and cyclohexanone, preferably 2-5 of them.
[0011] In any embodiment, the mixed organic solvent is formed by mixing several organic solvents with different boiling points in a certain proportion, namely, a low boiling point solvent, a medium boiling point solvent and a high boiling point solvent; wherein the low boiling point solvent has a boiling point less than 100°C, the medium boiling point solvent has a boiling point of 100-200°C, and the high boiling point solvent has a boiling point greater than 200°C.
[0012] In any embodiment, the mass fraction of the high boiling point organic solvent in the mixed solvent in the total slurry is greater than 10 wt %.
[0013] In any embodiment, the average particle size of the tantalum carbide solid powder particles is 1 μm-10 μm, and the purity is greater than 99%.
[0014] In any embodiment, the sintering aid is one or more of a reducing additive and a second phase additive.
[0015] In any embodiment, the reducing additive is TiB2, B4C, etc., and the second phase additive is SiC, WC, etc.
[0016] In any embodiment, the content of the sintering aid is 1-5wt% of the mass fraction of the tantalum carbide solid powder.
[0017] In any embodiment, the binder is an organic soluble binder, and the organic soluble binder is one or more of a vinyl binder, an acrylic binder, or a resin binder.
[0018] In any embodiment, the mass fraction of the mixed organic solvent in the total slurry is 20-50wt%. The mass fraction of the tantalum carbide solid powder particles in the total slurry is 50-80wt%; the mass fraction of the sintering aid solid powder particles in the total slurry is 0.5-3wt%; the mass fraction of the binder in the total slurry is 0.5-1wt%;
[0019] In any embodiment, after the slurry suspension is shaken and mixed evenly and then left to stand for 2-4 hours, no obvious solid-liquid boundary phenomenon between the solid powder particles and the liquid mixed organic solvent occurs; and after the slurry is dried, the bulk density of the powder can reach more than 70%.
[0020] The second aspect of the present application provides a sintering method for preparing a dense tantalum carbide coating, comprising the following steps: 1) uniformly coating the slurry on the graphite surface at room temperature; 2) placing the coated graphite part in a protective gas environment at 200-300°C for drying and curing for 1 hour; 3) placing the dried and cured tantalum carbide coated graphite part in a protective gas or vacuum environment at 2000-2500°C for sintering for 2-3 hours.
[0021] In any embodiment, a single coating process of the coating does not exceed 2 minutes, and the coating is left to dry after the single coating, which is repeated 3-5 times to obtain a tantalum carbide coating with a thickness of 50-100 μm.
[0022] In any embodiment, the heating rate of the drying and curing stage is 3-8°C / min; the heating rate of the sintering process is 5-15°C / min, and the high temperature maintenance time is 2-3 hours.
[0023] The present invention has the following advantages:
[0024] The tantalum carbide coating slurry prepared by the present invention has good suspension stability and is not easy to deposit, has good fluidity and is easy to apply, and has high coating film quality. The coating prepared by spraying the slurry has good adhesion to the substrate after drying, and does not crack or peel. The coating prepared by the sintering process is firmly bonded to the graphite substrate after high-temperature sintering, and its morphology shows high density when observed under an electron microscope. The slurry preparation and sintering process of the tantalum carbide coating of the present invention are simple, and can be used to prepare a tantalum carbide coating with high density, high bonding strength, and suitable thickness. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a physical picture of a slurry used to prepare a dense tantalum carbide coating in this application.
[0026] Figure 2 This is a photo of the actual tantalum carbide coating after spraying tantalum carbide slurry on the surface of graphite material and drying it.
[0027] Figure 3 This is a scanning electron microscope image of the surface of the tantalum carbide coating after spraying tantalum carbide slurry on the surface of graphite material and drying.
[0028] Figure 4 This is a photo of a tantalum carbide coating after sintering at 2400°C in an environment with argon protective gas, according to a sintering method for preparing a dense tantalum carbide coating in the present application.
[0029] Figure 5 This is a scanning electron microscope image of the surface of a tantalum carbide coating after sintering at a high temperature of 2400°C and in an environment with argon protective gas, according to a sintering method for preparing a dense tantalum carbide coating in the present application. DETAILED DESCRIPTION
[0030] Hereinafter, an embodiment of a slurry and a sintering method for preparing a dense tantalum carbide coating of the present application is specifically disclosed with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0031] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0032] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0033] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0034] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0035] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0036] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0037] The key to preparing tantalum carbide coating by slurry sintering method lies in the slurry preparation and sintering process of tantalum carbide. The preparation and sintering process of tantalum carbide slurry are directly related to the performance of tantalum carbide coating after sintering. Among them, the solvent composition used in the slurry is the key to limiting the dispersibility and solid content of the slurry. The solvent system of the existing slurry cannot achieve a slurry with good suspension stability and high solid content, and after sintering, it is impossible to prepare a tantalum carbide coating film with high bulk density, dense and flat surface, and strong bonding ability. At present, there is little research on the specific details of the slurry preparation and sintering process of tantalum carbide coating prepared by slurry sintering method. Therefore, the present invention focuses on the improvement of product performance by the specific details of tantalum carbide coating slurry and sintering process.
[0038] Reference Figure 1-3A slurry for preparing a dense tantalum carbide coating includes a volatile mixed organic solvent, tantalum carbide solid powder particles insoluble in the solvent, a sintering aid solid powder particles insoluble in the solvent, and a binder soluble in the solvent, which are mixed according to a certain mass fraction. The mixed suspension of the mixed raw material components is ball-milled to form a uniformly mixed suspension.
[0039] As an important component of the slurry, the solvent gives the slurry fluidity, allowing the powder to be evenly suspended in the liquid, and also evenly disperses various additive components to form a suspension mixture with high solid content and stable uniformity. Therefore, the main functions of the solvent are: 1) dissolving additives such as binders and plasticizers; 2) making the ceramic powder particles evenly dispersed; 3) providing the slurry with suitable viscosity and good fluidity. 4) can be dried volatile.
[0040] In any embodiment, the organic solvent is an organic solvent such as alcohol, ketone, etc., which has good wettability to tantalum carbide solid powder particles and can be suspended in it for a long time without sedimentation. It is preferably an organic solvent that can keep tantalum carbide solid powder particles suspended for 1-5 hours without sedimentation, such as ethanol, cyclohexanol, glycerol, acetone, cyclohexanone, etc. The longer the suspension time of tantalum carbide solid powder particles in the organic solvent, the higher the solid content of the coating slurry, the higher the bulk density of the tantalum carbide coating powder after spraying, and the higher the density after high-temperature sintering. Therefore, it is very necessary to select an organic solvent with a long suspension time of tantalum carbide solid powder particles.
[0041] In any embodiment, the organic solvent is a mixture of 2-5 organic solvents with different boiling points in a certain proportion. A single organic solvent cannot meet the subsequent gradient temperature drying process, and the use of a single organic solvent is very likely to cause stress cracking and peeling of the slurry surface. Therefore, the present application adopts a ternary or multi-component mixed solvent combination. The use of mixed organic solvents with different boiling points can control the drying rate of the wet tantalum carbide coating, and at the same time can reduce the drying stress during the coating drying process, and avoid cracking or peeling of the coating during the slurry drying process. According to the boiling point, organic solvents can be divided into low boiling point solvents, medium boiling point solvents and high boiling point solvents. The boiling point of the low boiling point solvent is less than 100°C, the boiling point of the medium boiling point solvent is 100-200°C, and the boiling point of the high boiling point solvent is greater than 200°C. The mass fraction of the high boiling point organic solvent in the mixed solvent to the total slurry is required to be greater than 10wt%, so as to avoid cracking or peeling of the coating in the subsequent drying process of the slurry.
[0042] In some embodiments, the average particle size of the tantalum carbide solid powder particles is 1 μm-10 μm, and the purity is greater than 99%. Experimental studies on the entire scheme found that the average particle size of tantalum carbide solid powder should not be greater than 10 μm. According to the principle of powder sintering densification, on the one hand, the larger the powder particle size, the larger the pores between the powder particles, which is not conducive to improving the density of the coating after sintering; on the other hand, the larger the powder particle size, the higher the diffusion activation energy required by the powder, which reduces the material diffusion and grain boundary diffusion on the surface of the powder particles, thereby reducing the density of the coating. At the same time, the average particle size of tantalum carbide solid powder should not be less than 1 μm. If the powder particle size is too small, during the high-temperature sintering densification process, the grains will grow abnormally or grow rapidly, so that the stress of the coating cannot be fully released, and peeling and cracking will occur.
[0043] In any embodiment, the sintering aid is one or more of a reducing additive and a second phase additive. The reducing additive is TiB2, B4C, etc., and the second phase additive is SiC, WC, etc. The reducing additive is TiB2, B4C, etc. Since the presence of oxygen elements will reduce the density of the coating, the addition of reducing additives can remove the oxygen elements in the slurry through a reduction reaction during high-temperature sintering, thereby increasing the density of the coating after sintering. The second phase additives include SiC, WC, etc. The addition of the second phase additive can reduce the temperature required for sintering densification, and can also inhibit excessive grain growth in the later stage of sintering, thereby increasing the density of the coating after sintering.
[0044] In any embodiment, the content of the sintering aid is 1-5wt% of the mass fraction of the tantalum carbide powder. The content of the sintering aid is 1-5wt% of the mass fraction of the tantalum carbide powder. The content of the sintering aid is required to be no less than 1wt% of the mass fraction of the tantalum carbide powder. Below this content, the density of the coating is not significantly improved. At the same time, the content of the sintering aid is required to be no more than 5wt% of the mass fraction of the tantalum carbide powder. If the content is too high, the bonding strength, thermal shock resistance and corrosion resistance of the tantalum carbide coating with graphite will decrease.
[0045] In any embodiment, the binder is an organic soluble binder. The binder has the greatest influence on the strength, plasticity, flexibility and smoothness of the slurry, and its type and content determine the strength and density of the coating. The selected binder should have the following characteristics: 1) It does not affect the volatilization of the solvent and does not generate bubbles; 2) It can prevent the particles from settling; 3) It is easy to burn off without leaving any residue; 4) It will not bond to the substrate. The organic soluble binder is one or more of a vinyl binder, an acrylic binder or a resin binder. Vinyl binders include polyvinyl alcohol (PVA), polyvinyl butyral (PVB), etc. Acrylic binders include polyacrylic acid (PAA), polymethyl methacrylate (PMMA), and polyethyl methacrylate (PEMA). Resin binders include epoxy acrylic resin (EA) and phenolic resin (PF). The binder is an important additive for tantalum carbide slurry. It wraps the powder in it, making the spacing between tantalum carbide powder particles smaller.
[0046] In any embodiment, the content of the binder is 0.5-1wt% of the mass fraction of the total slurry. The binder content should not be too low, otherwise the bonding effect between the powders will be poor, the bulk density of the powders after spraying will be low, and it will be unfavorable for the sintering and densification of the coating; similarly, the binder content should not be too high, otherwise the slurry will be viscous and the fluidity will be poor, which is not conducive to spraying and reduces the uniformity of the coating after spraying.
[0047] In any embodiment, the mass fraction of the mixed organic solvent in the total slurry is 20-50wt%. The mass fraction of the tantalum carbide solid powder particles in the total slurry is 50-80wt%; the mass fraction of the sintering aid solid powder particles in the total slurry is 0.5-3wt%; the mass fraction of the binder in the total slurry is 0.5-1wt%;
[0048] In any embodiment, after the slurry suspension is shaken and mixed evenly and then left to stand for 2-4 hours, no obvious solid-liquid boundary phenomenon between the solid powder particles and the liquid mixed organic solvent occurs; and after the slurry is dried, the bulk density of the powder can reach more than 70%.
[0049] Reference Figure 1-5 A sintering method for preparing a dense tantalum carbide coating comprises the following steps: 1) uniformly coating a slurry on a graphite surface at room temperature; 2) placing the coated graphite piece in a protective gas environment at 200-300°C for drying and curing for 1 hour; 3) placing the dried and cured tantalum carbide coated graphite piece in a protective gas or vacuum environment at 2000-2500°C for sintering for 2-3 hours.
[0050] The slurry is evenly coated on the graphite surface at room temperature (about 25°C) by methods including but not limited to spraying, dipping, scraping, and spin coating. Drying and curing treatment removes organic solvents and binders. The drying and curing temperature is required to be >200°C, otherwise the high-boiling point organic solvent cannot be fully volatilized and removed; the drying and curing temperature is required to be <300°C, otherwise the high-boiling point organic solvent is easily boiled, destroying the uniformity and flatness of the coating surface. Sintering for 2-3 hours allows the tantalum carbide solid powder to form a dense tantalum carbide coating under the action of high-temperature diffusion. The sintering temperature is required to be 2000-2500°C. If the coating is sintered below 2000°C, the sintering driving energy is low, and the low density of the coating is observed under an electron microscope; if the coating is sintered above 2500°C, the coating surface becomes black, and XRD test analysis shows that carbon peaks appear in the blackened area, and the coating is carbonized.
[0051] In any embodiment, a single coating process of the coating does not exceed 2 minutes, and the coating is left to dry after the single coating, which is repeated 3-5 times to obtain a tantalum carbide coating with a thickness of 50-100 μm.
[0052] A single coating process does not exceed 2 minutes; after a single coating, the coating is left to dry to evaporate the organic solvent and avoid uneven coating caused by liquid surface tension.
[0053] In any embodiment, the heating rate of the drying and curing stage is 3-8°C / min; the heating rate of the sintering process is 5-15°C / min, and the high temperature maintenance time is 2-3 hours.
[0054] The drying and curing stage requires slow heating (3-8℃ / min) to slowly release the stress of the coating to avoid cracking and peeling of the coating during the drying and curing stage; at the same time, the organic solvent inside the coating should not boil due to rapid heating to the boiling point, causing raised dots on the coating surface. The sintering atmosphere should be filled with protective gases such as argon or a vacuum environment. The sintering process requires a heating rate of 5-15℃ / min to slowly release the stress of the coating to avoid cracking or peeling of the coating due to a rapid heating rate.
[0055] Example
[0056] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0057] Embodiment 1:
[0058] Weigh 5g of tantalum carbide powder with a particle size of 1-3μm and a purity of 99.5%; weigh 0.2g of WC powder as a second phase sintering aid; weigh 0.05g of PVB powder as a binder; evenly mix the three organic solvents of ethanol, cyclohexanol and propylene glycol in a volume ratio of 2:2:1, and measure 4.75g as an organic solvent; mix the above four raw materials together and evenly ball mill to form a stable tantalum carbide slurry with good fluidity. The slurry is evenly coated on the graphite surface by spraying, and the coating is left to dry for a period of time after each spraying cycle, and this is repeated 3 times. After the spraying is completed, the graphite piece coated with tantalum carbide is placed in an environment of 300℃ and argon or other protective gas for drying and curing for 1 hour to remove the organic solvent and binder, and the heating rate in the drying and curing stage is 5℃ / min. Finally, the dried and cured tantalum carbide coated graphite piece is placed in a vacuum environment of 2400℃ for sintering for 2 hours, and the heating rate is 10℃ / min.
[0059] Embodiment 2:
[0060] Weigh 5g of tantalum carbide powder with a particle size of 1-3μm and a purity of 99.5%; weigh 0.2g of B4C powder as a reducing sintering aid; weigh 0.05g of phenolic resin powder as a binder; evenly mix the three organic solvents of ethylene glycol, cyclohexanone and propylene glycol in a volume ratio of 2:2:1, and measure 4.75g as an organic solvent; mix the above four raw materials together and ball mill them to form a stable tantalum carbide slurry with good fluidity. The slurry is evenly coated on the graphite surface by spraying, and the coating is left to dry for a period of time after each spraying cycle, and this is repeated 3 times. After the spraying is completed, the graphite part coated with tantalum carbide coating is placed in an environment of 300℃ and argon or other protective gas for drying and curing for 1 hour to remove the organic solvent and binder. The heating rate in the drying and curing stage is 5℃ / min. Finally, the dried and solidified tantalum carbide coated graphite parts were sintered in a vacuum environment at 2400°C for 2 hours with a heating rate of 10°C / min.
[0061] Embodiment three:
[0062] Weigh 5g of tantalum carbide powder with a particle size of 1-3μm and a purity of 99.5%; weigh 0.2g of TiB2 powder as a second phase sintering aid; weigh 0.05g of PAA powder as a binder; mix the three organic solvents of ethanol, cyclohexanone and propylene glycol in a volume ratio of 2:2:1, and measure 4.75g as an organic solvent; mix the above four raw materials together and ball mill them to form a stable tantalum carbide slurry with good fluidity. The slurry is evenly coated on the graphite surface by spraying, and the coating is left to dry for a period of time after each spraying cycle, and this is repeated 3 times. After the spraying is completed, the graphite parts coated with tantalum carbide coating are placed in an environment with argon and other protective gases at 300℃ for 1 hour to dry and cure, and the organic solvent and binder are removed. The heating rate in the drying and curing stage is 5℃ / min. Finally, the dried and cured tantalum carbide coated graphite parts are placed in a vacuum environment of 2400℃ for sintering for 2 hours, and the heating rate is 10℃ / min.
[0063] Figure 1 From left to right, the photos of the slurries prepared in Example 1 (1#), Example 2 (2#), and Example 3 (3#) are shown one by one, and it can be seen that the slurries are uniformly dispersed in the solvent; Figure 2 In Example 1, the slurry is sprayed on the surface of the graphite material. From the photo after drying, it can be seen that the coating on the graphite surface is evenly distributed, and the surface is flat and smooth without voids; Figure 3 In Example 1, the slurry is sprayed on the surface of the graphite material. From the scanning electron microscope photo of the surface after drying, it can be seen that in terms of microstructure, the solid powder of the slurry is distributed densely and evenly, and no obvious macroscopic voids appear; Figure 4 This is a photo of the actual object after the slurry is sprayed on the surface of the graphite material in Example 1 and sintered at 2400°C for 2 hours. It can be seen that the surface of the sample is smooth and uniform after sintering, without defects that can be distinguished by the naked eye, and the uniform color indicates that the thickness is uniform; Figure 5 This is an electron microscope photograph of the actual object after spraying the slurry on the surface of the graphite material in Example 1 and sintering at 2400°C for 2 hours. It can be seen that the coating after sintering is uniform and dense, and the surface is composed of densely stacked larger tantalum carbide grains, which proves that the slurry and sintering method of the present invention can prepare high-quality tantalum carbide coatings.
[0064] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A slurry for preparing a dense tantalum carbide coating, It is characterized in that The method comprises a mixed suspension of volatile organic solvents, tantalum carbide solid powder particles insoluble in the solvent, sintering aid solid powder particles insoluble in the solvent, and a binder soluble in the solvent, and ball milling the mixed raw material components to form a uniformly mixed suspension.
2. The slurry according to claim 1, It is characterized in that The average particle size of the tantalum carbide solid powder particles is 1 μm-10 μm, and the purity is greater than 99%.
3. The slurry according to claim 1, It is characterized in that The slurry suspension is shaken and mixed evenly and then left to stand for several hours without any obvious solid-liquid boundary between the solid powder particles and the liquid mixed organic solvent; and the bulk density of the powder after the slurry is dried can reach more than 70%.
4. The slurry according to claim 1, It is characterized in that The sintering aid is one or more of a reducing additive and a second phase additive; the reducing additive is TiB 2 , B 4 C, the second phase additive is SiC, WC; the content of the sintering aid is 1wt%-5wt% of the mass fraction of tantalum carbide powder.
5. The slurry according to claim 1, It is characterized in that The binder is an organic soluble binder, and the organic soluble binder is one of a vinyl binder, an acrylic binder or a resin binder; the content of the binder is 0.5-1wt% of the mass fraction of the total slurry.
6. The slurry according to claim 1, It is characterized in that The mixed organic solvent is a volatile mixed organic solvent, which is an alcohol or ketone solvent, and has good wettability to tantalum carbide solid powder particles and can be suspended in the solid powder particles for a long time without settling; the mixed organic solvent is at least two of ethanol, cyclohexanol, glycerol, acetone, and cyclohexanone.
7. The slurry according to claim 1, It is characterized in that The mass fraction of the tantalum carbide solid powder particles in the total slurry is 50-80wt%; the mass fraction of the sintering aid solid powder particles in the total slurry is 0.5-3wt%; the mass fraction of the binder solid powder particles in the total slurry is 0.5-1wt%; the mass fraction of the mixed organic solvent in the total slurry is 20-50wt%.
8. The slurry according to claim 1, It is characterized in that The mixed organic solvent is formed by mixing several organic solvents with different boiling points in a certain proportion, namely, a low boiling point solvent, a medium boiling point solvent and a high boiling point solvent; wherein the boiling point of the low boiling point solvent is less than 100°C, the boiling point of the medium boiling point solvent is 100-200°C, and the boiling point of the high boiling point solvent is greater than 200°C; the mass fraction of the high boiling point organic solvent in the mixed solvent is greater than 10wt% of the total slurry.
9. A sintering method for preparing a dense tantalum carbide coating, comprising the following steps: 1) uniformly coating a slurry on a graphite surface at room temperature; 2) placing the coated graphite piece in a protective gas environment at 200-300°C for drying and curing for 1 hour; 3) placing the dried and cured tantalum carbide coated graphite piece in a protective gas or vacuum environment at 2000-2500°C for 2-3 hours.
10. The slurry according to claim 1, It is characterized in that The single coating process of the coating does not exceed 2 minutes. After the single coating, the coating is left to dry, and the process is repeated 3-5 times to obtain a tantalum carbide coating with a thickness of 50-100 μm.
Citation Information
Patent Citations
Low-cost tantalum carbide coating preparation method
CN106699228A
Tantalum carbide coating, preparation method of tantalum carbide coating, carbonaceous structural member and application of carbonaceous structural member
CN117776781A
Tantalum carbide slurry, tantalum carbide coating, preparation method of tantalum carbide coating and crucible
CN118063214A
Production method of optical film, optical film and image display
US20070231478A1
Cited By
Method for preparing carbide coating with high bonding strength on graphite surface
CN121342554A
A tantalum carbide / pyrolytic graphite composite coating and its preparation method and application
CN122810648A