Preparation method of high-durability transparent cooling self-cleaning coating for stone cultural relic protection
By spraying multiple layers of nanoparticle mixed coatings on stone cultural relics, the problems of water erosion and high temperature and strong light damage in outdoor environments are solved, and coatings with high transparency, hydrophobicity and self-cleaning properties are achieved to ensure that Long-term protection of cultural relics.
Patent Information
- Application Number
- CN202411025892.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Stone cultural relics are susceptible to water erosion, pollution and high temperature and strong light in outdoor environments. The existing superhydrophobic coatings have shortcomings in transparency and durability, and it is difficult to provide effective protection without changing the appearance of cultural relics.
Using a high-durability transparent cooling self-cleaning coating for stone cultural relics protection, the combination of silica, titanium oxide and zinc oxide nanoparticles with silane coupling agent and aqueous emulsion is used to form hydrophobic and transparent The adhesive layer solution of large amounts of hydroxyl groups is formed on the surface of the cultural relics through ultrasonic spraying technology to ensure the chemical stability and mechanical stability of the coating.
It realizes that the coating with high transparency, hydrophobicity and self-cleaning properties without changing the appearance of the cultural relics. It has excellent chemical stability and mechanical stability, can effectively prevent cultural relics damage in high temperature and strong light environments, and is equipped with A certain heat resistance and cooling effect.
Smart Images

Figure HDA0004968516640000011 
Figure HDA0004968516640000012 
Figure HDA0004968516640000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a method for preparing a highly durable transparent cooling self-cleaning coating for protecting stone cultural relics. Background Art
[0002] Cultural relics are heritages of great value created by human beings in the long history of social history. Protecting cultural relics is to inherit the history of civilization development. Some stone cultural relics are exposed to the outdoor environment. Due to long-term exposure to various forms of water erosion in nature and the continuous accumulation of various pollutants and microorganisms on the surface, their appearance has changed significantly. Therefore, timely preventive protection of cultural relics is very important.
[0003] Superhydrophobic materials can repel water and most liquids, just like lotus leaves. When water droplets come into contact with the surface, they form a sphere and roll off the surface easily. Such surfaces usually have a contact angle greater than 150° and a sliding angle less than 10°, which prevents water droplets from spreading on the surface. This is because the surface has a microstructure with a certain degree of roughness and low surface energy, and there are many tiny protrusions on the surface, which can reduce the actual contact area between water droplets and the material. At the same time, the chemical composition of the surface is often hydrophobic, which further enhances the liquid repellency. In addition, the rough structure of superhydrophobic materials will increase the scattering of incident light and seriously reduce the light transmittance of the coating surface.
[0004] Some outdoor stone cultural relics are exposed to strong light and high temperature all year round, and their surfaces may experience cracks, discoloration and other appearance changes, so it is crucial to develop a super-hydrophobic coating with high transparency. Summary of the invention
[0005] To solve the above problems, the purpose of the present invention is to provide a method for preparing a highly durable, transparent, cooling and self-cleaning coating for the protection of stone cultural relics. The self-cleaning coating can provide preventive protection for the cultural relics without changing their original appearance, and has sufficient tolerance to mechanical damage and chemical invasion. It can effectively prevent damage to the cultural relics under high temperature and strong light, and has a strong cleaning performance for dust, dirt and other pollutants on the surface of the cultural relics.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a highly durable transparent cooling self-cleaning coating for protecting stone cultural relics comprises the following steps:
[0008] (1) Weighing silicon dioxide nanoparticles, titanium dioxide nanoparticles and zinc oxide nanoparticles in a mass ratio of 1:(0.5-1.5):(1-2) and dispersing them in a mixed solution of anhydrous ethanol and isopropanol in a volume ratio of 1:(1-1.5), and ultrasonicating for 15 minutes to obtain a mixed dispersion with a concentration of 1-10 mg / mL;
[0009] (2) Weighing 1 g of silica nanoparticles and dispersing them in a mixed solution of 10 mL of anhydrous ethanol and 10 mL of isopropanol, and ultrasonicating for 10-15 min to obtain a silica dispersion;
[0010] (3) Slowly adding a silane coupling agent and hydrochloric acid to the mixed dispersion and the silica dispersion, respectively, and then dropping a 5% ammonia solution to activate and modify the mixed dispersion and obtain a composite sol solution A and a single silica sol solution B after magnetic stirring;
[0011] (4) adding an aqueous emulsion diluted with water to the single silica sol solution B, wherein the mass of the aqueous emulsion is 3-4 times the mass of the single silica sol solution B, stirring for 0.5-1 hour and then ultrasonicating for 0.5-1 hour to obtain a bonding layer solution for spraying;
[0012] (5) spraying 20-80 layers of the obtained bonding layer solution on the sample after ultrasonic treatment, and naturally curing at room temperature for 0.5-1.5 hours;
[0013] (6) After ultrasonicating the composite sol solution A for 15 min, 200 layers are sprayed on the sample continuously and evenly using a spray gun with a moving speed of 2-4 cm / s;
[0014] (7) The sprayed sample was dried at room temperature for 1-3 days to obtain a transparent super-hydrophobic coating.
[0015] Preferably, the particle size of the silicon dioxide nanoparticles is 10-40 nm, the particle size of the titanium dioxide nanoparticles is 5-10 nm, and the particle size of the zinc oxide nanoparticles is 20-40 nm.
[0016] Preferably, the silane coupling agent in step (3) is diethoxydimethylsilane, and its mass is 3-4 times the total mass of the nanoparticles in the solution to be added, while the mass of hydrochloric acid is 0.5-1 times the total mass of the nanoparticles in the solution to be added, and the volume of the ammonia water added is 0.5%-1% of the total volume of the solution to be added.
[0017] Preferably, the stirring condition in step (3) is 25-30° C. at room temperature, and the stirring duration is 24-48 h.
[0018] Preferably, the aqueous emulsion in step (4) is styrene acrylic emulsion.
[0019] Preferably, the ultrasonic time in step (5) is 10-30 min.
[0020] Preferably, in step (6), the spraying pressure of the spray gun is 0.2 MPa, and the distance between the spray gun and the sample is 15-20 cm.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present application uses a diluted aqueous emulsion mixed with modified silica to form a hydrophobic adhesive substrate, and then a transparent protective coating formed by mixing a variety of nanoparticles. Styrene acrylic emulsion has good hydrophobicity and durability, and cures into a transparent state with high light transmittance at room temperature without heating or UV curing. The surface of silica is rich in a large number of hydroxyl groups and has a strong hydrophilicity, and the silane coupling agent diethoxydimethylsilane can reduce the hydroxyl groups on the surface of silica after hydrolysis, thereby increasing the hydrophobicity of silica. The coating has excellent hydrophobicity and oleophobicity and self-cleaning properties; it has excellent chemical stability and mechanical stability, has a certain heat resistance and cooling effect, and can produce liquid repellency to most liquids in life. The materials used are environmentally friendly and non-toxic, and can be widely used in various indoor and outdoor cultural relics for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a graph showing the water drop contact angle test results of the highly durable transparent cooling self-cleaning coating prepared in Example 1;
[0024] Figure 2 This is a comparison of the UV transmittance of high-durability transparent cooling self-cleaning coatings with different numbers of spray layers. The inset in the figure is a photo of different numbers of coatings on sandstone blocks;
[0025] Figure 3 This is an AFM image of the highly durable, transparent, cooling and self-cleaning coating prepared in Example 1;
[0026] Figure 4 This is a SEM image of the highly durable, transparent, cooling and self-cleaning coating prepared in Example 1;
[0027] Figure 5 Schematic diagram of the self-cleaning performance of the highly durable transparent cooling self-cleaning coating prepared in Example 1;
[0028] Figure 6 The graph showing the change in water drop contact angle and sliding angle of the highly durable transparent cooling self-cleaning coating prepared in Example 1 after the tape bonding cycle test;
[0029] Figure 7 The contact angle and sliding angle variation diagram of water droplets with different pH values on the surface of the high-durable transparent cooling self-cleaning coating prepared in Example 1;
[0030] Figure 8 These are the infrared temperature measurement results of Example 4 after the sandstone blocks were sprayed with different numbers of layers under strong light irradiation, from (a) to (d) are 0 layers, 200 layers, 300 layers, and 400 layers respectively. DETAILED DESCRIPTION
[0031] The present invention will be further described below in conjunction with specific embodiments.
[0032] Example 1
[0033] This embodiment provides a method for preparing a highly durable transparent cooling self-cleaning coating for protecting stone cultural relics, comprising the following steps:
[0034] (1) Weighing 2 g of silicon dioxide nanoparticles, 2 g of titanium dioxide nanoparticles, and 3 g of zinc oxide nanoparticles, dispersed them in a mixed solution of 20 mL of anhydrous ethanol and 20 mL of isopropanol, and ultrasonicated for 15 min to obtain a mixed dispersion with a concentration of 1-10 mg / mL;
[0035] (2) Weighing 1 g of silica nanoparticles and dispersing them in a mixed solution of 10 mL of anhydrous ethanol and 10 mL of isopropanol, and ultrasonicating for 15 min to obtain a dispersion containing only silica nanoparticles;
[0036] (3) slowly adding 24 g of diethoxydimethylsilane and 4 g of hydrochloric acid to the mixed dispersion, slowly adding 3.5 g of diethoxydimethylsilane and 0.6 g of hydrochloric acid to the silica dispersion, and then dropping 0.5 mL and 0.1 mL of 5% ammonia solution respectively for activation and modification, and magnetically stirring at room temperature for 24 h to obtain a composite sol solution A and a single silica sol solution B respectively;
[0037] (4) Add 4 g of styrene-acrylic emulsion diluted with water to the single silica sol solution B, stir for 1 hour and then ultrasonicate for 0.5 hour to obtain a bonding layer solution for spraying;
[0038] (5) spraying 40 layers of the obtained bonding layer solution on the sandstone block after ultrasonic treatment for 15 minutes, and naturally curing at room temperature for 0.5 hours;
[0039] (6) After ultrasonicating the composite sol solution A for 15 minutes, 200 layers were sprayed on the sandstone block. During the spraying, the spray gun was used to continuously and evenly spray the sandstone block with a moving speed of 2-4 cm / s. The spraying pressure of the spray gun was 0.2 MPa, and the distance between the spray gun and the sandstone block was 15-20 cm.
[0040] (7) The sprayed sandstone block was dried at room temperature for 24 h to obtain a transparent superhydrophobic coating.
[0041] The contact angle of the prepared coating was tested. The test results are shown in the attached figure. Figure 1 As shown in the figure, the contact angle is more than 150°. Figure 2 As shown, attached Figure 2 The light transmittance of the sandstone blocks sprayed with different numbers of layers is compared. It is easy to see that the light transmittance of the sandstone blocks sprayed with different numbers of layers is slightly lower than that of the unsprayed sandstone blocks, but it is maintained above 70%; Figure 3and attached Figure 4 Observation of the surface structure of the sandstone block shows that the nanoparticles are evenly distributed on the coating surface, forming a sufficiently rough structure; Figure 5 The figure is a schematic diagram of the self-cleaning performance of the transparent super-hydrophobic coating prepared on the sandstone block. Comparing the state of the sandstone block surface before and after cleaning, it can be proved that the coating has excellent self-cleaning performance. Water droplets rolling off the coating can easily carry away pollutants. Figure 6 For the tape adhesion test, the tape is repeatedly pasted on the coating surface and then torn off. After 30 cycles, the coating still has a water drop contact angle higher than 150°; Figure 7 The graph shows the contact angle test results of droplets with different pH values on the coating surface, which proves that the coating has excellent chemical stability.
[0042] Example 2
[0043] This embodiment provides a method for preparing a highly durable transparent cooling self-cleaning coating for protecting stone cultural relics, comprising the following steps:
[0044] (1) Weighing 1 g of silicon dioxide nanoparticles, 1 g of titanium dioxide nanoparticles, and 1.5 g of zinc oxide nanoparticles, dispersed them in a mixed solution of 10 mL of anhydrous ethanol and 10 mL of isopropanol, and ultrasonicated for 10 min to obtain a mixed dispersion;
[0045] (2) Weighing 1 g of silica nanoparticles and dispersing them in a mixed solution of 10 mL of anhydrous ethanol and 10 mL of isopropanol, and ultrasonicating for 10 min to obtain a dispersion containing only silica nanoparticles;
[0046] (3) Slowly adding 12 g of diethoxydimethylsilane and 2 g of hydrochloric acid to the mixed dispersion, slowly adding 3.5 g of diethoxydimethylsilane and 0.6 g of hydrochloric acid to the silica dispersion, and then dropping 0.2 mL and 0.1 mL of 5% ammonia solution respectively for activation and modification, and magnetically stirring at room temperature for 24 h to obtain a composite sol solution A and a single silica sol solution B respectively;
[0047] (4) adding 6 g of styrene-acrylic emulsion diluted with water to the single silica sol solution B, stirring for 1 hour and then ultrasonicating for 1 hour to obtain a bonding layer solution for spraying;
[0048] (5) spraying 30 layers of the obtained bonding layer solution on the sandstone block after ultrasonic treatment for 15 minutes, and naturally curing at room temperature for 0.5 hours;
[0049] (6) After ultrasonicating the composite sol solution A for 15 minutes, 150 layers were sprayed on the sandstone block continuously and evenly with a spray gun at a moving speed of 2-4 cm / s, the spraying pressure of the spray gun was 0.2 MPa, and the distance between the spray gun and the sandstone block was 15-20 cm;
[0050] (7) The sprayed sandstone block was dried at room temperature for 48 h to obtain a transparent superhydrophobic coating.
[0051] The prepared coating has a water contact angle of 158° and a maximum transmittance of 78% in the visible light range.
[0052] Example 3
[0053] This embodiment provides a method for preparing a highly durable transparent cooling self-cleaning coating for protecting stone cultural relics, comprising the following steps:
[0054] (1) Weighing 0.6 g of silicon dioxide nanoparticles, 0.6 g of titanium dioxide nanoparticles, and 0.9 g of zinc oxide nanoparticles, dispersed them in a mixed solution of 10 mL of anhydrous ethanol and 10 mL of isopropanol, and ultrasonicated for 15 min to obtain a mixed dispersion;
[0055] (2) Weighing 1 g of silica nanoparticles and dispersing them in a mixed solution of 10 mL of anhydrous ethanol and 10 mL of isopropanol, and ultrasonicating for 15 min to obtain a dispersion containing only silica nanoparticles;
[0056] (3) Slowly adding 7 g of diethoxydimethylsilane and 1 g of hydrochloric acid to the mixed dispersion, slowly adding 3.5 g of diethoxydimethylsilane and 0.6 g of hydrochloric acid to the silica dispersion, and then dropping 0.2 mL and 0.1 mL of 5% ammonia solution respectively for activation and modification, and magnetically stirring at room temperature for 24 h to obtain a composite sol solution A and a single silica sol solution B respectively;
[0057] (4) Add 6 g of styrene-acrylic emulsion diluted with water to the single silica sol solution B, stir for 1 hour and then ultrasonicate for 0.5 hour to obtain a bonding layer solution for spraying;
[0058] (5) spraying 60 layers of the obtained bonding layer solution on the sandstone block after ultrasonic treatment for 15 minutes, and naturally curing at room temperature for 0.5 hours;
[0059] (6) After ultrasonicating the composite sol solution A for 15 minutes, 200 layers were sprayed on the sandstone block. During the spraying, the spray gun was used to continuously and evenly spray the sandstone block with a moving speed of 2-4 cm / s. The spraying pressure of the spray gun was 0.2 MPa, and the distance between the spray gun and the sandstone block was 15-20 cm.
[0060] (7) The sprayed sandstone block was dried at room temperature for 24 h to obtain a transparent superhydrophobic coating.
[0061] The prepared transparent super-hydrophobic coating has a water contact angle of 160° and a maximum transmittance of 75% in the visible light range.
[0062] Example 4
[0063] This embodiment provides a method for preparing a highly durable transparent cooling self-cleaning coating for protecting stone cultural relics, comprising the following steps:
[0064] (1) Weighing 2 g of silicon dioxide nanoparticles, 1 g of titanium dioxide nanoparticles, and 2 g of zinc oxide nanoparticles, dispersed them in a mixed solution of 10 mL of anhydrous ethanol and 15 mL of isopropanol, and ultrasonicated for 10 min to obtain a mixed dispersion;
[0065] (2) Weighing 1 g of silica nanoparticles and dispersing them in a mixed solution of 10 mL of anhydrous ethanol and 15 mL of isopropanol, and ultrasonicating for 10 min to obtain a dispersion containing only silica nanoparticles;
[0066] (3) Slowly adding 17 g of diethoxydimethylsilane and 3 g of hydrochloric acid to the mixed dispersion, slowly adding 3.5 g of diethoxydimethylsilane and 0.6 g of hydrochloric acid to the silica dispersion, and then dropping 0.3 mL and 0.1 mL of 5% ammonia solution respectively for activation and modification, and magnetically stirring at room temperature for 24 h to obtain a composite sol solution A and a single silica sol solution B respectively;
[0067] (4) Add 4 g of styrene-acrylic emulsion diluted with water to the single silica sol solution B, stir for 1 hour and then ultrasonicate for 0.5 hour to obtain a bonding layer solution for spraying;
[0068] (5) spraying 60 layers of the obtained bonding layer solution on the sandstone block after ultrasonic treatment for 15 minutes, and naturally curing at room temperature for 0.5 hours;
[0069] (6) After ultrasonicating the composite sol solution A for 15 minutes, 200 layers were sprayed on the sandstone block. During the spraying, the spray gun was used to continuously and evenly spray the sandstone block with a moving speed of 2-4 cm / s. The spraying pressure of the spray gun was 0.2 MPa, and the distance between the spray gun and the sandstone block was 15-20 cm.
[0070] (7) The sprayed sandstone block was dried at room temperature for 24 h to obtain a transparent superhydrophobic coating.
[0071] The prepared transparent super-hydrophobic coating has a water contact angle of 156° and a maximum transmittance of 71% in the visible light range.
[0072] Example 5
[0073] This embodiment provides a method for preparing a highly durable transparent cooling self-cleaning coating for protecting stone cultural relics, comprising the following steps:
[0074] (1) Weighing 1 g of silicon dioxide nanoparticles, 1.5 g of titanium dioxide nanoparticles, and 2 g of zinc oxide nanoparticles, dispersed them in a mixed solution of 10 mL of anhydrous ethanol and 15 mL of isopropanol, and ultrasonicated for 10 min to obtain a mixed dispersion;
[0075] (2) Weighing 1 g of silica nanoparticles and dispersing them in a mixed solution of 10 mL of anhydrous ethanol and 15 mL of isopropanol, and ultrasonicating for 10 min to obtain a dispersion containing only silica nanoparticles;
[0076] (3) Slowly adding 15 g of diethoxydimethylsilane and 3 g of hydrochloric acid to the mixed dispersion, slowly adding 3.5 g of diethoxydimethylsilane and 0.6 g of hydrochloric acid to the silica dispersion, and then dropping 0.3 mL and 0.1 mL of 5% ammonia solution respectively for activation and modification, and magnetically stirring at room temperature for 24 h to obtain a composite sol solution A and a single silica sol solution B respectively;
[0077] (4) Add 4 g of styrene-acrylic emulsion diluted with water to the single silica sol solution B, stir for 1 hour and then ultrasonicate for 0.5 hour to obtain a bonding layer solution for spraying;
[0078] (5) spraying 80 layers of the obtained bonding layer solution on the sandstone block after ultrasonic treatment for 15 minutes, and naturally curing at room temperature for 0.5 hours;
[0079] (6) After ultrasonicating the composite sol solution A for 15 minutes, 200 layers were sprayed on the sandstone block. During the spraying, the spray gun was used to continuously and evenly spray the sandstone block with a moving speed of 2-4 cm / s. The spraying pressure of the spray gun was 0.2 MPa, and the distance between the spray gun and the sandstone block was 15-20 cm.
[0080] (7) The sprayed sandstone block was dried at room temperature for 24 h to obtain a transparent superhydrophobic coating.
[0081] The prepared transparent super-hydrophobic coating has a water contact angle of 157° and a maximum transmittance of 72% in the visible light range.
[0082] Example 6
[0083] This embodiment provides a method for preparing a highly durable transparent cooling self-cleaning coating for protecting stone cultural relics, comprising the following steps:
[0084] (1) Weighing 2 g of silicon dioxide nanoparticles, 2 g of titanium dioxide nanoparticles, and 3 g of zinc oxide nanoparticles, dispersed them in a mixed solution of 20 mL of anhydrous ethanol and 20 mL of isopropanol, and ultrasonicated for 15 min to obtain a mixed dispersion with a concentration of 1-10 mg / mL;
[0085] (2) Weighing 1 g of silica nanoparticles and dispersing them in a mixed solution of 10 mL of anhydrous ethanol and 10 mL of isopropanol, and ultrasonicating for 15 min to obtain a dispersion containing only silica nanoparticles;
[0086] (3) slowly adding 24 g of diethoxydimethylsilane and 4 g of hydrochloric acid to the mixed dispersion, slowly adding 3.5 g of diethoxydimethylsilane and 0.6 g of hydrochloric acid to the silica dispersion, and then dropping 0.5 mL and 0.1 mL of 5% ammonia solution respectively for activation and modification, and magnetically stirring at room temperature for 24 h to obtain a composite sol solution A and a single silica sol solution B respectively;
[0087] (4) Add 4 g of styrene-acrylic emulsion diluted with water to the single silica sol solution B, stir for 1 hour and then ultrasonicate for 0.5 hour to obtain a bonding layer solution for spraying;
[0088] (5) spraying 40 layers of the obtained bonding layer solution on the sandstone block after ultrasonic treatment for 15 minutes, and naturally curing at room temperature for 0.5 hours;
[0089] (6) After ultrasonicating the composite sol solution A for 15 min, the composite sol solution A was sprayed on three sandstone blocks, with the number of layers being 200, 300, and 400, respectively. During the spraying, the composite sol solution A was sprayed on the sandstone blocks continuously and evenly with a spray gun having a moving speed of 2-4 cm / s, a spray pressure of 0.2 MPa, and a distance between the spray gun and the sandstone blocks of 15-20 cm.
[0090] (7) The sprayed sandstone block was dried at room temperature for 24 h to obtain a transparent superhydrophobic coating.
[0091] The prepared transparent super hydrophobic coating has a water contact angle of 161° and a maximum transmittance of 70% in the visible light range. Infrared temperature measurement was performed on the high-durable transparent cooling self-cleaning coatings with different coatings prepared on sandstone blocks. The surface temperatures of the sandstone blocks with no coating, 200 layers of coating, 300 layers of coating and 400 layers of coating were 62.4°C, 60.4°C, 59.4°C and 57.7°C, respectively, indicating that the coating prepared by the present invention has a certain cooling effect on the protection of cultural relics, can effectively reduce the damage caused by high temperature and strong light to cultural relics, and is conducive to more comprehensive protection of cultural relics.
[0092] The above are all preferred embodiments of the present application, but not all embodiments, and the protection scope of the present application cannot be limited accordingly. Therefore, all equivalent changes made based on the products, methods, and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a highly durable transparent cooling self-cleaning coating for stone cultural relics protection, characterized in that: The following steps are involved: (1) Weighing silicon dioxide nanoparticles, titanium dioxide nanoparticles and zinc oxide nanoparticles in a mass ratio of (0.5-1-1.5):(1-1.5-2) and dispersing them in a mixed solution of anhydrous ethanol and isopropanol in a volume ratio of 1:(1-1.5), and ultrasonicating for 15 minutes to obtain a mixed dispersion with a concentration of 1-10 mg / mL; (2) Weighing 1 g of silica nanoparticles and dispersing them in a mixed solution of 10 mL of anhydrous ethanol and 10 mL of isopropanol, and ultrasonicating for 10-15 min to obtain a silica dispersion; (3) Slowly adding a silane coupling agent and hydrochloric acid to the mixed dispersion and the silica dispersion, respectively, and then dropping a 5% ammonia solution to activate and modify the mixed dispersion and obtain a composite sol solution A and a single silica sol solution B after magnetic stirring; (4) adding an aqueous emulsion diluted with water to the single silica sol solution B, wherein the mass of the aqueous emulsion is 3-4 times the mass of the single silica sol solution B, stirring for 0.5-1 hour and then ultrasonicating for 0.5-1 hour to obtain a bonding layer solution for spraying; (5) spraying 20-80 layers of the obtained bonding layer solution on the sample after ultrasonic treatment, and naturally curing at room temperature for 0.5-1.5 hours; (6) After ultrasonicating the composite sol solution A for 15 min, 200 layers are sprayed on the sample. During the spraying, a spray gun with a moving speed of 2-4 cm / s is used to continuously and evenly spray on the sample. (7) The sprayed sample is dried at room temperature for 1-3 days to obtain a transparent super-hydrophobic coating.
2. The method for preparing a highly durable transparent cooling self-cleaning coating for stone cultural relics protection according to claim 1, characterized in that: The particle size of the silicon dioxide nanoparticles is 10-40 nm, the particle size of the titanium dioxide nanoparticles is 5-10 nm, and the particle size of the zinc oxide nanoparticles is 20-40 nm.
3. The method for preparing a highly durable transparent cooling self-cleaning coating for stone cultural relics protection according to claim 1, characterized in that: The silane coupling agent in step (3) is diethoxydimethylsilane, and its mass is 3-4 times the total mass of the nanoparticles in the solution to be added, while the mass of hydrochloric acid is 0.5-1 times the total mass of the nanoparticles in the solution to be added, and the volume of the ammonia water added is 0.5%-1% of the total volume of the solution to be added.
4. The method for preparing a highly durable transparent cooling self-cleaning coating for stone cultural relics protection according to claim 1, characterized in that: The stirring condition in step (3) is 25-30° C. at room temperature, and the stirring duration is 24-48 h.
5. The method for preparing a highly durable transparent cooling self-cleaning coating for stone cultural relics protection according to claim 1, characterized in that: The aqueous emulsion in step (4) is styrene-acrylic emulsion.
6. The method for preparing a highly durable transparent cooling self-cleaning coating for stone cultural relics protection according to claim 1, characterized in that: The ultrasonic time in step (5) is 10-30 min.
7. The method for preparing a highly durable transparent cooling self-cleaning coating for stone cultural relics protection according to claim 1, characterized in that: In the step (6), the spraying pressure of the spray gun is 0.2 MPa, and the distance between the spray gun and the sample is 15-20 cm.
Citation Information
Patent Citations
Prepn process of nanometer composite titania / silica photocatalyst sol and transparent photocatalyzing film
CN101088606A
Super-hydrophobic nanometer transparent coating and preparation method thereof
CN104987520A
Superhydrophobicity coating based on waterborne emulsion and preparing method and application thereof
CN106433364A
Wetting-resisting super-hydrophobic membrane and preparation method thereof
CN109012199A
Method of preparing super-hydrophobic coating by compounding waterborne polyurethane and hydrophobic modified inorganic nanoparticles