Solvent-resistant UV moisture dual-curing polyurethane resin and preparation method thereof
Through the preparation method without solvent addition, the combination of temperature control and specific monomers is used to form a UV moisture dual-curing polyurethane resin with high NCO content, which solves the problems of insufficient curing and complex process in the prior art, and realizes high-density fat The ring structure and strong after-curing ability significantly improve the solvent resistance and toughness of the paint film.
Patent Information
- Application Number
- CN202411312866.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-27
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
AI Technical Summary
The existing UV moisture dual curing polyurethane resin is not cured sufficiently in opaque materials, complex shapes and super-thick coatings, and the use of organic solvents during the preparation process leads to complex process and health hazards. The polyurethane modified polyol is not resistant to alkaline liquids and Poor organic solvent compatibility leads to abnormal cured paint film.
Using the preparation method of solvent-free addition, the isocyanate reaction activity is controlled by introducing the first stage of temperature insulation to form a UV moisture dual-curing polyurethane resin with high NCO content, containing polyurea bonds and a large number of fat rings, ensuring post-curing ability and solvent resistance. , avoid the risk of explosive polymerization, and improve the toughness and invariance of the paint film through a combination of specific monomers and polymerization inhibitors.
UV moisture dual-curing polyurethane resin with high-density fat ring structure has strong post-curing ability, non-yellowing, wear resistance and toughness, simplifies the preparation process, avoids the hazards of solvent use, and significantly improves the paint film solvent resistance.
Smart Images

Figure CN118955861A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and in particular relates to a solvent-resistant UV moisture dual-curing polyurethane resin and a preparation method thereof. Background Art
[0002] Ultraviolet (UV) light curing has many advantages such as low volatile organic compound emissions, fast curing speed, and good comprehensive performance of the cured film, making it widely used internationally. However, UV light curing technology has certain defects, namely, deep curing is not good between opaque materials, on complex-shaped substrates, in ultra-thick coatings and colored coatings. Therefore, the use of UV light-dark dual curing technology can achieve thorough curing of the paint film. Moisture curing is a dark curing method commonly used in UV light-dark dual curing technology. The patent application with publication number CN110105530A provides a method for preparing UV moisture dual curing polyurethane resin. The method modifies polyester polyol with polyurethane, and reserves NCO bonds when using photocuring monomer hydroxy acrylate to cap the end to achieve post-curing. However, polyurethane-modified polyester polyol has serious solvent resistance problems, especially ester bonds are easily broken when in contact with alkali liquid. In addition, polyurethane-modified polyether polyol will also swell due to the compatibility of polyether segments with organic solvents, resulting in abnormal cured paint film. However, there are also methods for preparing UV moisture dual curing polyurethane resin without using polyols. The patent application with publication number CN109776755A directly uses hydroxy acrylate and diisocyanate at 60-105°C to prepare UV moisture dual curing polyurethane resin. The preparation process uses organic solvents to disperse the heat generated by polymerization to avoid the risk of explosion. The solvent needs to be removed after the reaction is completed, resulting in a complicated process for the entire preparation process. The use of organic solvents also poses a health hazard to production workers. Summary of the invention
[0003] Purpose of the invention: Based on the deficiencies of the prior art, the purpose of the present invention is to provide a solvent-resistant UV moisture dual-curing polyurethane resin and a preparation method thereof, wherein the preparation method does not require solvent addition and the preparation process is simple. The UV moisture dual-curing polyurethane resin prepared by the present invention has a high-density aliphatic ring structure and a high NCO content of up to 8-12%, and has a strong post-curing ability. By introducing the first-stage initiation temperature insulation, the reactivity of part of the isocyanate can be suppressed, and the risk of implosion in the preparation process can be effectively avoided. In addition, the polyurea bonds and a large number of aliphatic rings formed after curing provide excellent solvent resistance, and the cured paint film also has non-yellowing performance, wear resistance and toughness.
[0004] Technical solution: A method for preparing a solvent-resistant UV moisture dual-curing polyurethane resin of the present invention specifically comprises the following steps:
[0005] (1) adding a terminal hydroxyl acrylate monomer, a polymerization inhibitor, and an antioxidant to a reaction vessel, and stirring until the solid matter is completely dissolved;
[0006] (2) heating the reaction system to 80-100° C. and vacuum dehydrating for 1-3 hours;
[0007] (3) After dehydration is completed, the temperature is lowered to 40-50° C., and then diisocyanate monomer is added;
[0008] (4) After the addition is completed, the temperature is slowly raised to 75-80°C, and the first stage initiation temperature is kept warm for 1-3 hours;
[0009] (5) Raise the system temperature to 87-92°C for the second stage of heat preservation for 2-4 hours;
[0010] (6) After the reaction is completed, turn off the heating, cool down and discharge the material.
[0011] Furthermore, as a preferred embodiment, the terminal hydroxyl-containing acrylic acid ester monomer in step (1) is one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and N-hydroxyethyl acrylamide.
[0012] Furthermore, as a preferred embodiment, the molar ratio of the terminal hydroxyl-containing acrylate monomer in step (1) to the diisocyanate monomer in step (3) is 1:(2-4).
[0013] Furthermore, as a preferred embodiment, the inhibitor in step (1) is one or more of p-hydroxyanisole, tert-butylhydroquinone, and p-tert-butylcatechol; and the amount of the inhibitor added is 0.01% to 0.05% of the total mass.
[0014] Furthermore, as a preferred embodiment, the antioxidant in step (1) is 2,6-di-tert-butyl-4-methylphenol; and the amount of the antioxidant added is 0.1% to 0.5% of the total mass of the system.
[0015] Furthermore, as a preferred embodiment, the diisocyanate monomer in step (3) is one or more of isophorone diisocyanate, dicyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, xylene diisocyanate, cyclohexane dimethylene diisocyanate, and methylcyclohexyl diisocyanate.
[0016] Furthermore, as a preferred embodiment, the discharge temperature of step (6) is 50-55°C.
[0017] The present invention also provides a solvent-resistant UV moisture dual-curing polyurethane resin prepared by the above preparation method, the specific structure of which is shown in formula (I) or formula (II) or formula (III):
[0018]
[0019] In the structural formula: R1 is CH3 or H; R2 is O or NH; R3 is CH (2-4) ; R4 is a structural segment containing cyclohexane.
[0020] Beneficial effects:
[0021] (1) The solvent-resistant UV moisture dual-curing polyurethane resin prepared by the present invention has no solvent addition during the preparation process, and the preparation process is simple and safe;
[0022] (2) The solvent-resistant UV-moisture dual-curing polyurethane resin prepared by the present invention has a relatively high NCO content (8-12%) and strong post-curing ability;
[0023] (3) The solvent-resistant UV-moisture dual-curing polyurethane resin prepared by the present invention has a large aliphatic ring density, and the cured paint film is tough and resistant to solvent wiping and immersion. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the infrared spectrum of the raw materials used in the preparation process described in Example 1 and its product, the UV moisture dual-curing polyurethane resin. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Note: The addition amount of each component in all examples is in parts by mass.
[0027] Embodiment 1:
[0028] Add 160 parts of hydroxyethyl acrylate, 0.13 parts of p-hydroxyanisole, and 1.31 parts of 2,6-di-tert-butyl-4-methylphenol to the reaction bottle, stir until the solid is completely dissolved, heat to 90°C, vacuum dehydrate for 1.5 hours, then cool to below 50°C, add 275 parts of isophorone diisocyanate in portions, slowly heat to 75°C, keep warm at 75-80°C for 2 hours in the first stage, continue to heat to 90-92°C for 2.5 hours in the second stage, complete the reaction, cool to below 55°C and discharge to obtain the UV moisture dual-curing polyurethane resin of this embodiment.
[0029] Example 2
[0030] Add 160 parts of hydroxyethyl acrylate, 0.14 parts of p-hydroxyanisole, and 1.37 parts of 2,6-di-tert-butyl-4-methylphenol to the reaction bottle, stir until the solid is completely dissolved, heat to 80°C, vacuum dehydrate for 3 hours, then cool to below 50°C, add 275 parts of isophorone diisocyanate in portions, slowly heat to 75°C, keep warm at 75-80°C for 1 hour in the first stage, continue to heat to 87-90°C for 4 hours in the second stage, complete the reaction, cool to below 55°C and discharge to obtain the UV moisture dual-curing polyurethane resin of this embodiment;
[0031] Example 3
[0032] Add 180 parts of hydroxyethyl acrylate, 0.13 parts of p-hydroxyanisole, and 1.28 parts of 2,6-di-tert-butyl-4-methylphenol to the reaction bottle, stir until the solid is completely dissolved, heat to 100°C, vacuum dehydrate for 1 hour, then cool to below 50°C, add 275 parts of isophorone diisocyanate in portions, slowly heat to 80°C, keep warm at 75-80°C for 3 hours in the first stage, continue to heat to 90-92°C for 2 hours in the second stage, complete the reaction, cool to below 55°C and discharge to obtain the UV moisture dual-curing polyurethane resin of this embodiment;
[0033] Example 4
[0034] This embodiment is substantially the same as embodiment 1, except that the feed materials are 130.14 parts of hydroxyethyl methacrylate, 0.14 parts of p-hydroxyanisole, 1.36 parts of 2,6-di-tert-butyl-4-methylphenol, and 275 parts of isophorone diisocyanate;
[0035] Example 5
[0036] This embodiment is substantially the same as embodiment 1, except that the feed materials are 150 parts of hydroxyethyl methacrylate, 0.11 parts of p-hydroxyanisole, 1.08 parts of 2,6-di-tert-butyl-4-methylphenol, and 210 parts of isophorone diisocyanate;
[0037] Comparative Example 1
[0038] Add 500 parts of polyester diol (hydroxyl equivalent is 500g / mol) to the reaction bottle, heat to 100°C, vacuum dehydrate for 1.5 hours, cool to room temperature, add 0.2 parts of dibutyltin dilaurate, increase the temperature, control the temperature at 45-50°C, add 275 parts of isophorone diisocyanate dropwise, and continue to keep warm for 30 minutes after the dripping is completed within 1.5 hours, then add 0.26 parts of p-hydroxyanisole and 2.58 parts of 2,6-di-tert-butyl-4-methylphenol in the reactor, stir until the solid is completely dissolved, increase the temperature, control the temperature at 50-55°C, add 85 parts of hydroxyethyl acrylate dropwise, and continue to keep warm for 30 minutes after the dripping is completed within 1 hour, increase the temperature, and keep warm at 68-75°C for 2 hours. After the reaction is completed, cool to below 55°C to discharge; obtain comparative sample 1.
[0039] Comparative Example 2
[0040] This comparative example is basically the same as comparative example 1, except that the feed materials are 500 parts of polyether diol (hydroxyl equivalent is 800 g / mol), 0.2 parts of dibutyltin dilaurate, 275 parts of isophorone diisocyanate, 0.26 parts of p-hydroxyanisole, and 2.57 parts of 2,6-di-tert-butyl-4-methylphenol.
[0041] In order to verify the NCO content and performance of the solvent-resistant UV moisture dual-curing polyurethane resin of the present invention, Examples 1-5 and Comparative Examples 1-2 were subjected to NCO content test, solvent resistance wiping test and solvent resistance immersion test, and the test method was as follows:
[0042] Resin NCO content test:
[0043] According to standard HG / T 2409-1992;
[0044] Solvent resistance wipe test:
[0045] 100 parts of UV moisture dual-curing polyurethane resin, 2 parts of photoinitiator TPO, and 2 parts of photoinitiator 184 were stirred and mixed evenly, and a 100 μm thick paint film was applied using an applicator. 2 Curing under energy conditions, leaving it at room temperature for 1-2 days until moisture curing is complete, then use non-woven cloth to dip in alcohol and acetone respectively, wipe back and forth on the surface of the paint film 500 times, and observe whether there are any abnormalities on the surface of the paint film, including surface cracking, surface dissolution, etc.
[0046] Solvent immersion test:
[0047] The UV moisture dual-curing polyurethane resin paint film was cured according to the above method, and then immersed in anhydrous ethanol and 5% sodium hydroxide solution for 14 days to observe whether the paint film has any abnormalities, including paint film dissolution, paint film swelling, paint film cracking, etc. The test results are shown in Table 1:
[0048] Table 1 Performance test results of products obtained from Examples 1-5 and Comparative Examples 1-2
[0049]
[0050]
[0051] From the results in Table 1, it can be seen that the NCO content of all embodiments of the present invention is relatively high, all of which are 8-12%. Due to the strong post-curing ability and the large amount of polyurea bonds contained after curing, the paint films of the embodiments are tough, and all embodiments have no abnormalities in the solvent wiping and solvent immersion tests, which is attributed to the large amount of aliphatic rings contained in the structure, providing excellent solvent resistance. The comparative example uses a diol oligomer as a modifier. Although the cured paint film performs well in the solvent wiping test, it is abnormal in the solvent immersion test. Due to the linear structure of the diol oligomer, the comparative examples swell in the solvent immersion, and the comparative example 1 cracks into a large number of fragments after swelling in a 5% sodium hydroxide solution, which is caused by the hydrolysis of the polyester block by alkali.
[0052] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.
Claims
1. A method for preparing a solvent-resistant UV moisture dual-curing polyurethane resin, characterized in that The steps include: (1) adding a terminal hydroxyl acrylate monomer, a polymerization inhibitor, and an antioxidant to a reaction vessel, and stirring until the solid matter is completely dissolved; (2) heating the reaction system to 80-100° C. and vacuum dehydrating for 1-3 hours; (3) After dehydration is completed, the temperature is lowered to 40-50° C., and then diisocyanate monomer is added; (4) After the addition is completed, the temperature is slowly raised to 75-80°C, and the first stage initiation temperature is kept warm for 1-3 hours; (5) Raise the system temperature to 87-92°C for the second stage of heat preservation for 2-4 hours; (6) After the reaction is completed, turn off the heating, cool down and discharge the material.
2. The method for preparing the solvent-resistant UV moisture dual-curing polyurethane resin according to claim 1, characterized in that: The terminal hydroxyl-containing acrylic acid ester monomer in step (1) is one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and N-hydroxyethyl acrylamide.
3. The method for preparing the solvent-resistant UV moisture dual-curing polyurethane resin according to claim 1, characterized in that: The molar ratio of the terminal hydroxyl-containing acrylate monomer in step (1) to the diisocyanate monomer in step (3) is 1:(2-4).
4. The method for preparing the solvent-resistant UV moisture dual-curing polyurethane resin according to claim 3, characterized in that: The inhibitor in step (1) is one or more of p-hydroxyanisole, tert-butylhydroquinone, and p-tert-butylcatechol; the amount of the inhibitor added is 0.01% to 0.05% of the total mass.
5. The method for preparing the solvent-resistant UV moisture dual-curing polyurethane resin according to claim 3, characterized in that: The antioxidant in step (1) is 2,6-di-tert-butyl-4-methylphenol; the amount of the antioxidant added is 0.1% to 0.5% of the total mass of the system.
6. The method for preparing the solvent-resistant UV moisture dual-curing polyurethane resin according to claim 3, characterized in that: The diisocyanate monomer in step (3) is one or more of isophorone diisocyanate, dicyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, xylylene diisocyanate, cyclohexane dimethylene diisocyanate, and methylcyclohexyl diisocyanate.
7. The method for preparing the solvent-resistant UV moisture dual-curing polyurethane resin according to claim 1, characterized in that: The discharge temperature of step (6) is 50-55°C.
8. A solvent-resistant UV moisture dual-curing polyurethane resin prepared by the preparation method according to any one of claims 1 to 7, wherein the specific structure is as shown in formula (I) or formula (II) or formula (III): In the structural formula: R1 is CH3 or H; R2 is O or NH; R3 is CH (2-4) ; R4 is a structural segment containing cyclohexane.
Citation Information
Patent Citations
Preparation method of UV moisture double curing resin
CN109776755A
Preparing method of UV moisture dual-cured resin
CN110105530A