Nitrogen-rich composite COF material as well as preparation method and application thereof
A nitrogen-rich composite COF material was prepared by loading imidazole onto COF-300, which solved the synthesis and adsorption kinetics problems of existing COF materials in gaseous iodine adsorption, and achieved a highly efficient iodine adsorption effect, which is convenient for large-scale application.
Patent Information
- Application Number
- CN202411305177.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing COF materials suffer from difficulties in monomer synthesis, demanding preparation conditions, and slow adsorption kinetics in gaseous iodine adsorption, which limits their large-scale application.
A nitrogen-rich composite COF material was prepared by loading covalent organic framework material COF-300 with imidazole. The high specific surface area and open pore structure of COF-300, combined with an electron-rich π-π conjugated system, enabled rapid iodine adsorption.
The preparation method is simple, the reaction conditions are mild, and it can achieve rapid adsorption of gaseous iodine, which is convenient for large-scale preparation and practical application, and the adsorption capacity is significantly improved.
Smart Images

Figure CN118955935A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the fields of environmental science, material science and synthesis technology, and in particular to a nitrogen-rich composite COF material and a preparation method and application thereof. Background Art
[0002] Radioactive iodine is an extremely important pollutant in gaseous radioactive nuclear waste due to its volatility, biocompatibility and high mobility. Once it leaks into the environment, it will cause great harm. Therefore, the research and development of efficient iodine adsorption materials is of great significance.
[0003] Solid phase adsorption is the most commonly used method for enriching and storing radioactive gas iodine and has been widely studied and applied. Covalent organic framework (COF) materials are a new type of crystalline porous polymer materials. Due to their highly flexible molecular designability and pore structure controllability, they have great research value and application prospects in the design and preparation of gaseous iodine adsorption materials. However, in existing studies, the use of COF materials for the uptake of gaseous iodine has the following problems: the monomers used are difficult to synthesize, the preparation of the target COF material requires a strict inert atmosphere and a high reaction temperature, the adsorption kinetics of iodine are slow, and it is not conducive to large-scale preparation and practical application. Summary of the invention
[0004] The purpose of the present invention is to provide a nitrogen-rich composite COF material and a preparation method and application thereof, so as to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] The present invention provides a method for preparing a nitrogen-rich composite COF material, comprising the following steps:
[0007] The covalent organic framework material COF-300 is used to load imidazole to obtain the nitrogen-rich composite COF material.
[0008] As a further preferred embodiment of the present invention, the mass ratio of the covalent organic framework material to imidazole is (0.8-0.2):1.
[0009] As a further preferred embodiment of the present invention, the load temperature is 120° C.; the load time is 24-72 hours.
[0010] As a further preferred embodiment of the present invention, the covalent organic framework material COF-300 is obtained by reacting tetrakis(4-aminophenyl)methane and terephthalaldehyde as monomers at 100°C.
[0011] As a further preferred embodiment of the present invention, the reaction time is 1-3 days.
[0012] As a further preferred embodiment of the present invention, the molar ratio of tetrakis(4-aminophenyl)methane (TAMA) to terephthalaldehyde (TA) is 3:5.
[0013] The structure of tetrakis(4-aminophenyl)methane is as follows:
[0014]
[0015] The structure of terephthalaldehyde is as follows:
[0016]
[0017] The structure of the prepared COF-300 is as follows:
[0018]
[0019] The more specific preparation method of the present invention is as follows:
[0020] The organic monomers tetrakis(4-aminophenyl)methane and terephthalaldehyde are mixed according to a molar ratio, ground, and placed in a heat-resistant glass tube, followed by the addition of anhydrous dioxane and acetic acid solution. The concentration of the acetic acid solution is preferably 3 mol / L, and the volume ratio of anhydrous dioxane to the acetic acid solution is preferably 5:1.
[0021] The heat-resistant glass tube was frozen in liquid nitrogen for 5-20 minutes, then vacuumed in the frozen state, and then refilled with nitrogen. After repeating the operation several times, the heat-resistant glass tube was sealed with a hydrogen-oxygen flame in a vacuum state. The sealed heat-resistant glass tube was placed at 100°C for 3 days, and the obtained block solid was ground and washed with N,N-dimethylformamide and tetrahydrofuran in turn. After drying at room temperature, it was vacuum dried at 100-150°C for 6 hours to obtain an orange-yellow powder, which is COF-300.
[0022] The prepared COF-300 was soaked in tetrahydrofuran for 24 h, filtered and vacuumed at 150 °C for 2 h, and the pre-weighed open vial containing COF-300 was placed in a larger sealed glass bottle containing imidazole. After sealing, it was heated in an oven at 120 °C for 24-72 h and cooled to room temperature to obtain a nitrogen-rich composite COF material (Im@COF material).
[0023] The present invention also provides a nitrogen-rich composite COF material prepared by the above preparation method.
[0024] The present invention further provides the use of the nitrogen-rich composite COF material as an iodine adsorbent.
[0025] The present invention discloses the following technical effects:
[0026] The present invention utilizes the covalent organic framework material COF-300 to load imidazole rich in nitrogen atoms to obtain a nitrogen-rich composite COF material. The nitrogen-rich composite COF material has a high specific surface area and an open pore structure. The nitrogen-rich structure and the electron-rich π-π conjugated system can provide effective binding sites for the adsorption of iodine. At the same time, the presence of a large number of nitrogen atoms can ensure the material's ability to adsorb iodine.
[0027] The preparation method of the nitrogen-rich composite COF material of the present invention is simple, the reaction conditions are mild, and the gaseous iodine can be quickly adsorbed, which is convenient for large-scale preparation and practical application. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is the powder X-ray diffraction (PXRD) pattern of COF-300.
[0030] Figure 2 This is the Fourier transform infrared spectrum (FTIR) of COF-300.
[0031] Figure 3 This is the loading amount of imidazole on COF material COF-300 and activated carbon.
[0032] Figure 4 These are the test results of the iodine adsorption performance of the four Im@COF materials prepared in Examples 1-4.
[0033] Figure 5 These are the experimental results of iodine adsorption performance of Im_0.075@COF-300 and COF-300 prepared in Example 3.
[0034] Figure 6 These are the static I2 vapor adsorption kinetic experimental results of Im_0.075@COF-300 prepared in Example 3.
[0035] Figure 7 The iodine retention test results (room temperature conditions) of the four Im@COF materials prepared in Examples 1-4 and a single COF sample COF-300 in a closed environment.
[0036] Figure 8The iodine retention test results (room temperature conditions) of the four Im@COF materials prepared in Examples 1-4 and a single COF sample COF-300 in a semi-enclosed environment.
[0037] Fig. 9 The iodine retention test results (room temperature conditions) of the four Im@COF materials prepared in Examples 1-4 and a single COF sample COF-300 in an open environment.
[0038] Fig.10 These are the experimental results of CH3I adsorption performance of Im_0.075@COF-300 and COF-300 prepared in Example 3. DETAILED DESCRIPTION
[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0040] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0044] Example 1
[0045] The organic monomer tetrakis(4-aminophenyl)methane (0.11mmol, 40mg) and terephthalaldehyde (0.18mmol, 24mg) were fully mixed and ground, and then loaded into a heat-resistant glass tube. Anhydrous dioxane and acetic acid solution (3mol / L) were then added to the glass tube in sequence, wherein the volume ratio of anhydrous dioxane to acetic acid solution was 5:1, and a total of 2.5mL was added.
[0046] The heat-resistant glass tube was frozen in liquid nitrogen for 15 minutes, then vacuumed in a frozen state, and then refilled with nitrogen. After repeating the operation three times, the heat-resistant glass tube was sealed with a hydrogen-oxygen flame in a vacuum state. The sealed heat-resistant glass tube was placed at 100°C for 3 days, and the obtained block solid was ground and washed with N,N-dimethylformamide and tetrahydrofuran in turn, dried at room temperature, and vacuum dried at 120°C for 6 hours to obtain an orange-yellow powder, which was marked as COF-300.
[0047] The prepared COF-300 was soaked in tetrahydrofuran for 24 h, filtered and vacuumed at 150 °C for 2 h, a pre-weighed open vial (20 mL) containing 20 mg COF-300 was placed in a larger sealed glass bottle (100 mL) containing 25 mg imidazole, sealed and heated in an oven at 120 °C for 72 h, cooled to room temperature, and the prepared product was labeled Im_0.025@COF-300.
[0048] Figure 1 This is the powder X-ray diffraction (PXRD) pattern of COF-300.
[0049] Figure 2 The FTIR spectrum of COF-300 shows that the C=O group and NH2 group disappear. The presence of C=N stretching vibration bond indicates that the Schiff base reaction forms an imine bond.
[0050] Example 2
[0051] The only difference from Example 1 is that the amount of imidazole added to the 100 mL sealed glass bottle is 50 mg. The prepared product is marked as Im_0.050@COF-300.
[0052] Example 3
[0053] The only difference from Example 1 is that the amount of imidazole added to the 100 mL sealed glass bottle is 75 mg. The prepared product is marked as Im_0.075@COF-300.
[0054] Example 4
[0055] The only difference from Example 1 is that the amount of imidazole added to the 100 mL sealed glass bottle is 100 mg. The prepared product is marked as Im_0.100@COF-300.
[0056] Comparative Example 1
[0057] The difference from Example 1 is that the imidazole is loaded with activated carbon (AC) equal to that of COF-300:
[0058] The activated carbon was soaked in tetrahydrofuran for 24 h, filtered and vacuumed at 150 ° C for 2 h, and a pre-weighed vial (20 mL) containing 20 mg of activated carbon was placed in a larger sealed glass bottle (100 mL) containing 25 mg of imidazole. After sealing, it was heated in an oven at 120 ° C for 72 h and cooled to room temperature to obtain activated carbon loaded with imidazole.
[0059] Comparative Example 2
[0060] The difference from Example 2 is that the imidazole is loaded with activated carbon (AC) in an amount equal to that of COF-300. The preparation method is the same as that of Comparative Example 1.
[0061] Comparative Example 3
[0062] The difference from Example 3 is that the imidazole is loaded with activated carbon (AC) in an amount equal to that of COF-300. The preparation method is the same as that of Comparative Example 1.
[0063] Comparative Example 4
[0064] The difference from Example 4 is that the imidazole is loaded with activated carbon (AC) in an amount equal to that of COF-300. The preparation method is the same as that of Comparative Example 1.
[0065] The loading amount of imidazole on COF material COF-300 and activated carbon is as follows Figure 3 As shown. Figure 3 It can be seen that when the amount of imidazole added is 75 mg, the imidazole loading of the COF material reaches the maximum value, and the corresponding product is Im_0.075@COF-300 synthesized in Example 3, and the imidazole loading energy of the COF material COF-300 is much higher than that of activated carbon.
[0066] Effect verification example 1: Static iodine vapor adsorption experiment
[0067] (1) I2 adsorption experiment
[0068] An open glass vial (20 mL) containing Im@COF was placed in a glass vial (100 mL) containing solid iodine, sealed and heated at 75°C. After a certain period of time, the sample bottle was cooled to room temperature and weighed, and then placed back into the iodine-containing bottle for continued adsorption until the weight of the sample bottle reached equilibrium, that is, the maximum iodine capture capacity was achieved.
[0069] Iodine absorption capacity is calculated by weight method: W = (m t -m0) / m×100%, where W is the iodine absorption capacity; m0 is the original weight of the sample bottle, g; m t is the weight of the sample bottle after iodine vapor adsorption, g; m is the weight of the COF sample, g.
[0070] (2) CH3I adsorption experiment
[0071] An open glass vial (20 mL) containing Im@COF was placed in a glass vial (100 mL) containing methyl iodide (CH3I), sealed and heated at 75°C. After a certain period of time, the sample bottle was cooled to room temperature and weighed, and then placed back into the iodine-containing bottle to continue adsorption until the weight of the sample bottle reached equilibrium, that is, the maximum CH3I capture capacity was achieved. The absorption capacity calculation method is consistent with the I2 adsorption experiment.
[0072] Figure 4 These are the test results of the iodine adsorption performance of the four Im@COF materials prepared in Examples 1-4.
[0073] Figure 5 These are the experimental results of iodine adsorption performance of Im_0.075@COF-300 prepared in Example 3 and COF sample COF-300.
[0074] according to Figure 4-Figure 5 It can be seen that the Im_0.075@COF-300 prepared in Example 3 has the best iodine adsorption effect, with an adsorption amount of up to 10.61 g / g, which is 1.9 times higher than the iodine adsorption of the COF-300 sample before loading with imidazole.
[0075] Figure 6 The results of the static I2 vapor adsorption kinetics experiment of Im_0.075@COF-300 prepared in Example 3. The iodine adsorption amount of the Im_0.075@COF-300 sample increased rapidly in the first 24 hours, and the adsorption curve was basically linear, and the adsorption curve tended to equilibrium after 24 hours.
[0076] Figure 7 The iodine retention test results (room temperature conditions) of the four Im@COF materials prepared in Examples 1-4 and a single COF sample COF-300 in a closed environment.
[0077] Figure 8The iodine retention test results (room temperature conditions) of the four Im@COF materials prepared in Examples 1-4 and a single COF sample COF-300 in a semi-enclosed environment.
[0078] Fig. 9 The iodine retention test results (room temperature conditions) of the four Im@COF materials prepared in Examples 1-4 and a single COF sample COF-300 in an open environment.
[0079] Depend on Figure 7-Figure 9 It can be seen that under three different environments, except that the iodine retention rate of Im_0.025@COF-300 in a semi-closed environment is slightly lower than that of COF-300, the iodine retention rates of other imidazole-loaded Im@COF-300 samples are higher than that of the single COF sample.
[0080] Fig.10 The experimental results of CH3I adsorption performance of Im_0.075@COF-300 and COF sample COF-300 prepared in Example 3. The results show that the adsorption effect of Im_0.075@COF-300 sample on CH3I is better than that of COF-300, and the adsorption amount increases from 0.61g / g to 1.04g / g, which is 1.7 times higher.
[0081] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a nitrogen-rich composite COF material, characterized in that: The following steps are involved: The covalent organic framework material COF-300 is used to load imidazole to obtain the nitrogen-rich composite COF material.
2. The method for preparing the nitrogen-rich composite COF material according to claim 1, characterized in that: The mass ratio of the covalent organic framework material COF-300 and imidazole is (0.8-0.2):
1.
3. The method for preparing the nitrogen-rich composite COF material according to claim 1, characterized in that: The load temperature is 120° C. and the load time is 24-72 hours.
4. The method for preparing the nitrogen-rich composite COF material according to claim 1, characterized in that: The covalent organic framework material COF-300 is obtained by reacting tetrakis(4-aminophenyl)methane and terephthalaldehyde as monomers at 100°C.
5. The method for preparing the nitrogen-rich composite COF material according to claim 4, characterized in that: The reaction time is 1-3 days.
6. The method for preparing the nitrogen-rich composite COF material according to claim 4, characterized in that: The molar ratio of tetrakis(4-aminophenyl)methane to terephthalaldehyde is 3:
5.
7. The nitrogen-rich composite COF material prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the nitrogen-rich composite COF material as claimed in claim 7 as an iodine adsorbent.
Citation Information
Patent Citations
Method used for adsorbing iodine with covalent organic framework material
CN106693601A
Covalent organic framework material based on secondary amine bonding, and preparation method and application thereof
CN108503853A
Functional organic porous polymer as well as preparation method and application thereof
CN112724373A
Application of imidazole / metal organic framework composite material
CN115382343A
Perylene bisimide / covalent organic framework composite fluorescent probe as well as preparation method and application thereof
CN118027324A