Radioactive organic waste liquid adsorption material and preparation method thereof

Adsorbent materials prepared by block crosslinking polymerization technology solve the problems of low adsorption ratio and pollution in the treatment of radioactive organic waste liquids in the prior art, achieving efficient and environmentally friendly adsorption effects, ensuring the firmness and safety of the material .

CN118930708AActive Publication Date: 2024-11-12EAST CHINA UNIV OF TECH

Patent Information

Application Number
CN202410997240.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The prior art cannot effectively treat radioactive organic waste liquids, especially the problems of low adsorption rate, slow absorption rate, non-flammable and contaminated.

Method used

Block cross-linking polymerization of short-chain aryl polymer monomers, long-chain alkane non-aromatic monomers, short-chain non-aromatic monomers, cross-linking agents and foaming agents is prepared to produce high absorption magnification, firmness and resistance. Adsorbent materials with pressure performance can achieve fine regulation of radioactive organic waste liquid by regulating the monomer ratio and polymerization conditions.

Benefits of technology

It achieves high absorption rate, firmness and environmentally friendly adsorbent materials, avoids pollution, and ensures the safe treatment and transportation of radioactive organic waste liquid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930708A_ABST
    Figure CN118930708A_ABST
Patent Text Reader

Abstract

The invention discloses a radioactive organic waste liquid adsorbing material and a preparation method thereof. The adsorbing material is prepared from the following raw materials: a short-chain aryl polymeric monomer A, a long-chain alkane non-aryl monomer B, a short-chain non-aryl monomer C, a cross-linking agent E, an initiator F and a foaming agent G, the mass ratio of the short-chain aryl polymeric monomer A to the long-chain alkane non-aryl monomer B to the short-chain non-aryl monomer C to the cross-linking agent E to the foaming agent G is 1: (0.1-10): (0.1-10): (0.01-0.2): (0.05-0.2). The radioactive organic waste liquid adsorption material provided by the invention has the characteristics of high absorption rate, strong firmness, large volume reduction ratio after combustion, displayability, easiness in combustion, no pollution to the environment in the combustion process and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nuclear waste treatment, and more particularly to a radioactive organic waste liquid adsorption material and a preparation method thereof. Background Art

[0002] The normal operation, maintenance, and decommissioning of nuclear facilities generate a large amount of radioactive organic waste liquid (such as TBP / kerosene solution, liquid scintillator, etc.). In addition to its physical and chemical properties such as flammability, explosiveness, volatility, thermal decomposition, biodegradability, and irradiation decomposition, radioactive organic waste liquid also contains radioactive nuclides such as uranium, plutonium, cerium, strontium, cesium, and cobalt. Therefore, efficient treatment of radioactive organic waste liquid is an important guarantee for the safe decommissioning of nuclear facilities.

[0003] The existing treatment methods are mainly high-temperature and high-pressure oxidation methods. For example, the direct combustion method is to directly burn the organic solvent to convert the macromolecular organic matter into small molecules of carbon dioxide, water and nitrogen oxides, and then absorb the small molecular compounds and solidify the residues. This method involves liquid combustion, the batch processing capacity is limited, and the chemical reaction during the incineration process is violent. Another example is the supercritical water oxidation method, that is, the organic solvent is oxidized in the supercritical water phase, and the residue is solidified. The reaction process conditions of this method are high temperature and high pressure, and the risk factor is relatively high.

[0004] In addition, CN202110493247.1 also proposed a radioactive organic solvent system solution of "adsorption solidification-barreling and transportation-solidified body incineration-residue solidification treatment", in which the radioactive organic solvent solidifier (i.e., radioactive organic waste liquid adsorption material) is the key to the solution. CN201910722997.4 discloses a polymer adsorbent and a preparation method thereof, which is mainly polymerized from halogen-containing olefin monomers, olefin-containing ester monomers, and olefin-containing cross-linking monomers. The polymer adsorbent can be used to treat surface oil leaks, hazardous organic liquid leaks, etc., but the adsorbent contains halogens such as Cl or Br, and is not easy to incinerate after adsorbing organic solvents. CN201310067847.7 and CN201210178912.9 respectively disclose a method for preparing a three-dimensional interconnected macroporous graphene high-efficiency oil-absorbing material and a biodegradable polyurethane oil-absorbing material and its preparation method. Such oil-absorbing materials have abundant interconnected pores and an adsorption rate of oils of up to dozens of times, but have large pore sizes and poor retention capacity for radioactive organic waste liquids with low viscosity, and cannot meet transportation requirements.

[0005] Therefore, how to provide an adsorption material with high adsorption ratio, fast absorption rate, strong adsorption, flammability and environmental protection is a problem that technical personnel in this field need to solve urgently. Summary of the invention

[0006] In view of this, the present invention prepares a flammable adsorption material with high adsorption ratio, fast absorption rate, selective adsorption of organic solvents, firm adsorption and so on for radioactive organic waste liquid.

[0007] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: 11. A radioactive organic waste liquid adsorption material, whose raw materials include: short-chain aromatic polymerization monomer A, long-chain alkane non-aromatic monomer B, short-chain non-aromatic monomer C, cross-linking agent E, initiator F, and foaming agent G; the mass ratio of the short-chain aromatic polymerization monomer A, long-chain alkane non-aromatic monomer B, short-chain non-aromatic monomer C, cross-linking agent E, and foaming agent G is 1: (0.1-10): (0.1-10): (0.01-0.2): (0.05-0.2).

[0008] The beneficial effects of adopting the above technical scheme are as follows: the monomer used in the present invention has a high volume reduction ratio and a pollution-free combustion process, avoiding the use of monomers containing halogen, nitrogen, phosphorus, etc. that are flame retardant and corrosive or pollute the environment after combustion. The present invention achieves fine regulation of the polymer's adsorption performance and firm retention capacity for different organic radioactive waste liquids through block cross-linking polymerization of aromatic long-chain monomers A, aromatic short-chain monomers B, and alkyl long-chain monomers C and cross-linking agents, and improves the absorption rate by adding a foaming agent. In addition, the adsorption material prepared by the present invention is a lipophilic porous spherical particle with a certain compressive resistance, and can selectively adsorb an organic phase.

[0009] The present invention achieves a balance between the absorption rate and firmness of the material by systematically regulating the dosage of each monomer and the polymerization conditions, and ensures that no secondary leakage occurs after the radioactive organic waste liquid is adsorbed while ensuring a high absorption rate.

[0010] Preferably, the short-chain aromatic polymer monomer A is selected from 2,5-dimethylalkenylbenzene, 2-allylphenol, allyl o-cresyl ether, allyl phenoxyacetate, allyl benzoate, allyl 4-hydroxybenzoate, 1-allyl-2-methylbenzene, terbinaphthol hydrochloride, allylbenzene, eugenol, styrene, distilbenes, 1-allyl-2-methylbenzene, triphenylethylene, benzyl propylene nitrile or tetraphenylethylene.

[0011] Preferably, the long-chain alkane non-aromatic monomer B is selected from allyl acetoacetate, butyl acrylate, hexadecyl acrylate, dodecene, octadecene, octadecyl acrylate, 4-pentanoic acid, allyl hexanoate, geraniol, myrcene, sorbic acid, ocimene, squalene, ricinoleic acid, ethyl oleate or oleic acid.

[0012] Preferably, the short-chain non-aromatic monomer C is selected from isoprene, diallylamine, allylthiourea, allyl acetate, norbornene, allyl nitrile, vinyl acetate or vinyl ethyl ether.

[0013] Preferably, the crosslinking agent E is selected from 1,3-dienylbenzene, divinylbenzene, triallylphosphine, triallylamine, 1,3-butadiene, 1,7-octadiene, isoprene, geranyl acetate or diallyl carbonate.

[0014] Preferably, the initiator F is selected from benzoyl peroxide, azobisisobutyronitrile, potassium persulfate or dicumyl peroxide.

[0015] Preferably, the foaming agent G is selected from sodium dodecyl sulfate, calcium carbonate, ammonium carbonate or urea.

[0016] Preferably, it further comprises a developer D, wherein the developer D is Sudan III or Sudan IV, and the mass ratio of the developer D to the short-chain aromatic polymerization monomer A is (0.005-0.01):1.

[0017] The beneficial effects of adopting the above technical solution are as follows: adding the color developer D makes the material present different colors when absorbing organic waste liquid at different ratios, and by comparing with the standard color developing card, visual identification of the absorption ratio can be achieved.

[0018] The present invention also discloses a method for preparing the above radioactive organic waste liquid adsorbent, comprising the following steps:

[0019] (1) mixing short-chain aromatic monomer A, long-chain alkane non-aromatic monomer B, short-chain non-aromatic monomer C, cross-linking agent E, and color developer D uniformly for use;

[0020] (2) adding the mixed solution obtained in step (1) to a polyvinyl alcohol solution containing an initiator F and a foaming agent G, heating under stirring conditions to carry out a cross-linking reaction, filtering to remove the solvent, and washing with deionized water to obtain a spherical particle radioactive organic waste liquid adsorbent material.

[0021] Preferably, the cross-linking reaction is carried out by heating to (60-100° C.), and the reaction is terminated after (6-12) hours.

[0022] It can be known from the above technical scheme that, compared with the prior art, the present invention discloses a radioactive organic waste liquid adsorption material with high absorption rate, firm retention, large volume reduction ratio after combustion, and display performance. The present invention adjusts the type and content of the foaming agent to adjust the pore size, volume and shape of the adsorption material to increase the adsorption rate of organic waste liquid; by adjusting the number, length and other factors of the alkyl substituents in the polymerized monomer, the adsorption firmness of the organic solvent is improved to meet the transportation requirements and avoid the leakage of radioactive organic waste liquid caused by the bumps during transportation; by adjusting the proportion of monomers A, B, and C, the relationship between their compressive resistance and adsorption performance is balanced; the proportion of crosslinking agent E and foaming agent G can adjust the density of the material, which is of great significance to prevent secondary oil leakage on the basis of ensuring the adsorption capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0024] Figure 1 The colors of the adsorption material prepared in Example 1 at different adsorption rates;

[0025] a: no adsorption; b: adsorption ratio 1:1; c: adsorption ratio 1:2; d: adsorption ratio 1:3; e: excessive adsorption;

[0026] Figure 2 The surface morphology and internal pore size state of the adsorption material prepared in Examples 1-4;

[0027] A: Example 1; B: Example 2; C: Example 3; D: Example 4;

[0028] Figure 3 The colors of the adsorption material prepared in Example 1 at different adsorption rates;

[0029] A: adsorption ratio 1:1; B: adsorption ratio 1:1.5; C: adsorption ratio 1:2. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] (1) 162.2 g of allyl benzoate, 168.3 g of n-dodecene, 215.3 g of vinyl acetate, 15 g of Sudan III, and 8.11 g of isoprene were stirred and mixed uniformly for use.

[0033] (2) The above mixed solution was added to a polyvinyl alcohol (mass fraction 0.2%) solution containing 27g of azobisisobutyronitrile as an initiator and 25g of sodium dodecyl sulfonate as a foaming agent, and heated to 80°C under stirring to carry out a crosslinking reaction. The reaction was terminated after 8 hours, and the solvent was removed by filtration. The product was washed with a large amount of deionized water to obtain spherical porous particles. After drying, it turned light pink, with a small amount of pores in the spheres, and the pore diameter was about 1.5-2 microns. Figure 2 (A) shown.

[0034] (3) Take 10g of the dried spherical product and place it in a sample bottle. Add tributyl phosphate solution containing radioactive elements (uranium mass fraction is 0.05%) in a ratio of 1:1, 1:1.5, and 1:2, let it stand, and observe the adsorption and color change. When the adsorbent mass / organic waste liquid mass = 1:1, the adsorption can be completed in only 4 minutes, the volume increase rate is 23%, there is no free organic waste liquid, and the color is lighter; when the adsorbent mass / organic waste liquid mass = 1:1.5, the complete adsorption time is 10 minutes, the volume increase rate is 35%, there is no free organic waste liquid, and the color is darker; when the adsorbent mass / organic waste liquid mass = 1:2, the complete adsorption time is 20 minutes, the volume increase rate is 42%, and there is a small amount of free organic waste liquid at the bottom, but the adsorption can be completed with slight stirring, and the solution color is darker at this time.

[0035] (4) Weigh 2 g of completely adsorbed adsorption materials with adsorption ratios of 1, 1.5, and 2, respectively, and place them in a crucible. Heat them to 800°C in a muffle furnace for pyrolysis (the time from room temperature to 800°C is about 1 h. After keeping the temperature for 2 h, observe the morphology of the residue, weigh it, and calculate the volume reduction ratio. The mass volume reduction ratios are 99.1%, 99.3%, and 99.5%, respectively.

[0036] (5) Weigh 2 g of fully adsorbed adsorbent materials with adsorption ratios of 1, 1.5, and 2, respectively, and place them in a φ2 cm × 3 cm organic glass mold (with a piece of filter paper placed above and below), pressurize to 50 psi and maintain for 30 seconds, and observe whether the waste liquid seeps out from the filter paper. The experimental results show that under a pressure of 50 psi, the adsorbent materials with adsorption ratios of 1, 1.5, and 2, respectively, have no waste liquid seeping out (such as Figure 3 When the pressure increases to 80psi, the material with an adsorption ratio of 2 begins to seep out a little; when the pressure increases to 100psi, the material with an adsorption ratio of 1.5 begins to seep out a little; when the pressure increases to 130psi, the material with an adsorption ratio of 1 begins to seep out a little.

[0037] Example 2

[0038] (1) Stir and mix 562.5 g of styrene, 421.2 g of butyl acrylate, 205.1 g of vinyl ethyl ether, 12 g of Sudan III, and 28.1 g of isoprene, a cross-linking agent, and set aside.

[0039] (2) The above mixed solution was added to a polyvinyl alcohol solution (mass fraction 0.2%) containing 22g of azobisisobutyronitrile as an initiator and 21g of sodium dodecyl sulfonate as a foaming agent, and heated to 80°C under stirring to carry out a crosslinking reaction. The reaction was terminated after 8 hours, and the solvent was filtered out. The product was washed with a large amount of deionized water to obtain spherical porous particles. After drying, it turned light pink, and there were many pores in the spheres, with a pore diameter of about 2-3 microns. Figure 2 (B) shown.

[0040] (3) Take 10g of the dried spherical product and place it in a sample bottle. Add tributyl phosphate solution containing radioactive elements (uranium mass fraction is 0.05%) in a ratio of 1:1, 1:1.5, and 1:2, and observe the adsorption and color change. When the adsorbent mass / organic waste liquid mass = 1:1, the adsorption can be completed in only 3 minutes, the volume increase rate is 21%, there is no free organic waste liquid, and the color is lighter; when the adsorbent mass / organic waste liquid mass = 1:1.5, the complete adsorption time is 10 minutes, the volume increase rate is 30%, there is no free organic waste liquid, and the color is darker; when the adsorbent mass / organic waste liquid mass = 1:2, the complete adsorption time is 20 minutes, the volume increase rate is 40%, and there is a small amount of free organic waste liquid at the bottom, but the adsorption can be completed with slight stirring, and the solution color is darker at this time.

[0041] (4) Weigh 2 g of completely adsorbed adsorption materials with adsorption ratios of 1, 1.5, and 2, respectively, and place them in a crucible. Heat them to 800°C in a muffle furnace for pyrolysis (the time from room temperature to 800°C is about 1 h. After keeping the temperature for 2 h, observe the morphology of the residue, weigh it, and calculate the volume reduction ratio. The mass volume reduction ratios are 98.2%, 98.7%, and 99.2%, respectively.

[0042] (5) Weigh 2g of fully adsorbed adsorbent materials with adsorption ratios of 1, 1.5, and 2, respectively, and place them in a φ2cm×3cm organic glass mold (with a piece of filter paper placed above and below), pressurize to 50psi and maintain for 30s, and observe whether the waste liquid on the filter paper seeps out. The experimental results show that under a pressure of 50psi, the adsorbent materials with adsorption ratios of 1, 1.5, and 2 have no waste liquid seepage. When the pressure increase value is 70psi, the material with an adsorption ratio of 2 begins to seep out a small amount; when the pressure increase value is 90psi, the material with an adsorption ratio of 1.5 begins to seep out a small amount; when the pressure increase value is 110psi, the material with an adsorption ratio of 1 begins to seep out a small amount.

[0043] Example 3

[0044] (1) 460.5 g of triphenylethylene monomer, 452.1 g of ethyl oleate monomer, 205.1 g of vinyl ethyl ether monomer, 12.2 g of Sudan IV color development agent, and 23 g of 1,3-butadiene crosslinking agent were stirred and mixed uniformly for use.

[0045] (2) The above mixed solution was added to a polyvinyl alcohol solution (mass fraction 0.3%) containing 22g of azobisisobutyronitrile as an initiator and 21g of sodium dodecyl sulfonate as a foaming agent, and heated to 80°C under stirring to carry out a crosslinking reaction. The reaction was terminated after 8 hours, and the solvent was filtered out. The product was washed with a large amount of deionized water to obtain spherical porous particles. After drying, it turned light pink, and there were many pores in the spheres, with a pore diameter of about 3-4 microns. Figure 2 (C) shown.

[0046] (3) Take 10g of the dried spherical product and place it in a sample bottle. Add tributyl phosphate solution containing radioactive elements (uranium mass fraction is 0.05%) in a ratio of 1:1, 1:1.5, and 1:2, and observe the adsorption and color change. When the adsorbent mass / organic waste liquid mass = 1:1, the adsorption can be completed in only 6 minutes, the volume increase rate is 20%, there is no free organic waste liquid, and the color is lighter; when the adsorbent mass / organic waste liquid mass = 1:1.5, the complete adsorption time is 12 minutes, the volume increase rate is 36%, there is no free organic waste liquid, and the color is darker; when the adsorbent mass / organic waste liquid mass = 1:2, the complete adsorption time is 30 minutes, the volume increase rate is 41%, and there is a small amount of free organic waste liquid at the bottom, but it can be completed by slight stirring, and the solution color is darker at this time.

[0047] (4) Weigh 2 g of completely adsorbed adsorption materials with adsorption ratios of 1, 1.5, and 2, respectively, and place them in a crucible. Heat them to 800°C in a muffle furnace for pyrolysis (the time from room temperature to 800°C is about 1 h. After keeping the temperature for 2 h, observe the morphology of the residue, weigh it, and calculate the volume reduction ratio. The mass volume reduction ratios are 98.4%, 98.9%, and 99.4%, respectively.

[0048] (5) Weigh 2g of fully adsorbed adsorbent materials with adsorption ratios of 1, 1.5, and 2, respectively, and place them in a φ2cm×3cm organic glass mold (with a piece of filter paper placed above and below), pressurize to 50psi and maintain for 30s, and observe whether the waste liquid on the filter paper seeps out. The experimental results show that under a pressure of 50psi, the adsorbent materials with adsorption ratios of 1, 1.5, and 2 have no waste liquid seepage. When the pressure increase value is 60psi, the material with an adsorption ratio of 2 begins to seep out a small amount; when the pressure increase value is 80psi, the material with an adsorption ratio of 1.5 begins to seep out a small amount; when the pressure increase value is 100psi, the material with an adsorption ratio of 1 begins to seep out a small amount.

[0049] Example 4

[0050] (1) 363.5 g of tetraphenylethylene, 350.1 g of oleic acid, 102.2 g of vinyl acetate, 5.2 g of Sudan IV, and 18.2 g of cross-linking agent isoprene are stirred and mixed uniformly for use.

[0051] (2) The above mixed solution was added to a polyvinyl alcohol solution (mass fraction 0.3%) containing 14g of azobisisobutyronitrile as an initiator and 12g of sodium dodecyl sulfonate as a foaming agent, and heated to 80°C under stirring to carry out a crosslinking reaction. The reaction was terminated after 8 hours, and the solvent was filtered out. The product was washed with a large amount of deionized water to obtain spherical porous particles. After drying, it turned light pink, with a small amount of pores in the spheres, and the pore diameter was about 4 microns. Figure 2 (D) as shown.

[0052] (3) Take 10g of the dried spherical product and place it in a sample bottle. Add tributyl phosphate solution containing radioactive elements (uranium mass fraction is 0.05%) in a ratio of 1:1, 1:1.5, and 1:2, and observe the adsorption and color change. When the adsorbent mass / organic waste liquid mass = 1:1, the adsorption can be completed in only 7 minutes, the volume increase rate is 22%, there is no free organic waste liquid, and the color is lighter; when the adsorbent mass / organic waste liquid mass = 1:1.5, the complete adsorption time is 15 minutes, the volume increase rate is 33%, there is no free organic waste liquid, and the color is darker; when the adsorbent mass / organic waste liquid mass = 1:2, the complete adsorption time is 30 minutes, the volume increase rate is 39%, and there is a small amount of free organic waste liquid at the bottom, but it can be completed by slight stirring, and the solution color is darker at this time.

[0053] (4) Weigh 2 g of completely adsorbed adsorption materials with adsorption ratios of 1, 1.5, and 2, respectively, and place them in a crucible. Heat them to 800°C in a muffle furnace for pyrolysis (the time from room temperature to 800°C is about 1 h. After keeping the temperature for 2 h, observe the morphology of the residue, weigh it, and calculate the volume reduction ratio. The mass volume reduction ratios are 98.5%, 99.1%, and 99.5%, respectively.

[0054] (5) Weigh 2g of fully adsorbed adsorbent materials with adsorption ratios of 1, 1.5, and 2, respectively, and place them in a φ2cm×3cm organic glass mold (with a piece of filter paper placed above and below), pressurize to 50psi and maintain for 30s, and observe whether the waste liquid on the filter paper seeps out. The experimental results show that under a pressure of 50psi, the adsorbent materials with adsorption ratios of 1 and 1.5 have no waste liquid seepage, and the adsorbent material with an adsorption ratio of 2 has a small amount of waste liquid seepage. When the pressure increase value is 60psi, the material with an adsorption ratio of 1.5 begins to seep out a small amount; when the pressure increase value is 80psi, the material with an adsorption ratio of 1 begins to seep out a small amount.

[0055] During the research and development process, the present invention firstly adds only short-chain aromatic polymer monomer A and long-chain alkane non-aromatic monomer B, and then optimizes the ratio of monomers A and B. As the ratio of monomer B increases from 0.1 to 1, the adsorption performance of the polymer increases. When A:B=2, the saturated adsorption capacity reaches a maximum value of 12g / g, and then the adsorption capacity decreases significantly with the increase of monomer B content (2-10). However, the compression resistance of the two-component material is poor. When the adsorption capacity is 1g / g, leakage occurs when the pressure reaches 20psi. In order to obtain excellent firm performance, after continuous experiments, it is found that when the third component monomer C is added, when the mass ratio of monomers A and B is fixed at 2, the adsorption capacity of component C and component A increases from 0.1 to 1. When A:B:C=1:2:1, the saturated adsorption capacity reaches a maximum value of 10g / g. Then, as the content of C increases (1-10), the adsorption capacity decreases. At this time, the compressive performance of the three-component material was significantly improved. When the adsorption amount was 1.5g / g, the pressure reached 50psi without leakage. Finally, by adjusting the ratio of crosslinking agent E and foaming agent G, after optimization, when the adsorption amount was 2g / g, the pressure reached 50psi and it could still maintain firm adsorption without leakage.

[0056] The present invention can identify the adsorption ratio by color. The materials after adsorbing waste liquid at different ratios have different colors. The adsorption ratio can be judged by comparing with the standard colorimetric card, which is of great significance in the leakage treatment process (in the event of a leak, the leaked liquid cannot be weighed, and more adsorbent is wasted, while less adsorbent is easily squeezed and leaked again during transportation).

[0057] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0058] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A radioactive organic waste liquid adsorption material, characterized in that: The raw materials include: short-chain aromatic polymerization monomer A, long-chain alkane non-aromatic monomer B, short-chain non-aromatic monomer C, cross-linking agent E, initiator F, and foaming agent G; the mass ratio of the short-chain aromatic polymerization monomer A, long-chain alkane non-aromatic monomer B, short-chain non-aromatic monomer C, cross-linking agent E, and foaming agent G is 1: (0.1-10): (0.1-10): (0.01-0.2): (0.05-0.2).

2. The radioactive organic waste liquid adsorption material according to claim 1, characterized in that: The short-chain aromatic polymer monomer A is selected from 2,5-dimethylalkenylbenzene, 2-allylphenol, allyl o-cresyl ether, allyl phenoxyacetate, allyl benzoate, allyl 4-hydroxybenzoate, 1-allyl-2-methylbenzene, terbinaphthol hydrochloride, allylbenzene, eugenol, styrene, distyrene, 1-allyl-2-methylbenzene, triphenylethylene, benzyl propylene dinitrile or tetraphenylethylene.

3. The radioactive organic waste liquid adsorption material according to claim 1, characterized in that: The long-chain alkane non-aromatic monomer B is selected from allyl acetoacetate, butyl acrylate, hexadecyl acrylate, dodecene, octadecene, octadecyl acrylate, 4-pentanoic acid, allyl hexanoate, geraniol, myrcene, sorbic acid, ocimene, squalene, ricinoleic acid, ethyl oleate or oleic acid.

4. The radioactive organic waste liquid adsorption material according to claim 1, characterized in that: The short-chain non-aromatic monomer C is selected from isoprene, diallylamine, allylthiourea, allyl acetate, norbornene, allyl nitrile, vinyl acetate or vinyl ethyl ether.

5. The radioactive organic waste liquid adsorption material according to claim 1, characterized in that: The crosslinking agent E is selected from 1,3-dienylbenzene, divinylbenzene, triallylphosphine, triallylamine, 1,3-butadiene, 1,7-octadiene, isoprene, geranyl acetate or diallyl carbonate.

6. The radioactive organic waste liquid adsorption material according to claim 1, characterized in that: The initiator F is selected from benzoyl peroxide, azobisisobutyronitrile, potassium persulfate or dicumyl peroxide.

7. The radioactive organic waste liquid adsorption material according to claim 1, characterized in that: The foaming agent G is selected from sodium dodecyl sulfonate, calcium carbonate, ammonium carbonate or urea.

8. The radioactive organic waste liquid adsorption material according to claim 1, characterized in that: It also includes a developer D, which is Sudan III or Sudan IV; the mass ratio of the developer D to the short-chain aromatic polymerization monomer A is (0.005-0.01):

1.

9. The method for preparing a radioactive organic waste liquid adsorbent according to claims 1-8, characterized in that: The following steps are involved: (1) mixing short-chain aromatic monomer A, long-chain alkane non-aromatic monomer B, short-chain non-aromatic monomer C, cross-linking agent E, and color developer D uniformly for use; (2) adding the mixed solution obtained in step (1) to a polyvinyl alcohol solution containing an initiator F and a foaming agent G, heating under stirring conditions to carry out a cross-linking reaction, filtering to remove the solvent, and washing with deionized water to obtain a spherical particle radioactive organic waste liquid adsorbent material.

10. The method for preparing a radioactive organic waste liquid adsorbent according to claim 1, characterized in that: Heat to (60-100°C) for cross-linking reaction, and terminate the reaction after (6-12) hours.

Citation Information

Patent Citations

  • High oil absorption resin and synthetic method thereof

    CN101215355A

  • Grease absorption porous material and preparation method thereof

    CN106977645A

  • Oil absorption and color development resin and preparation method thereof

    CN108017748A

  • High-oil-absorption resin capable of rapidly adsorbing oil products and preparation method thereof

    CN113896829A

  • Uranium adsorption resin as well as preparation method and application thereof

    CN116178607A

Cited By

  • Method for absorbing and curing radioactive organic waste liquid at low cost by using styrene block polymer

    CN122627523A