High-weather-resistance biodegradable mulching film and preparation method thereof

By using hollow nanotube materials to load anti-aging additives in biodegradable plastic films, the problem of poor weather resistance of biodegradable plastic films is solved, and the anti-aging performance and service life of plastic films are significantly improved.

CN118955972APending Publication Date: 2024-11-15INST OF BIOLOGICAL & MEDICAL ENG GUANGDONG ACAD OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411200133.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The poor weather resistance of biodegradable plastic films leads to a decrease in product performance with the increase of use time, and small additive molecules are unevenly dispersed in the material and are easy to migrate, making them unable to maintain weather resistance for a long time.

Method used

By chemical grafting and physical adsorption of hollow nanotube materials with anti-aging additives, high weather resistance additives are prepared and mixed with poly(terephthalic acid-butylene adipate)/polylactic acid and other materials, extrusion is used Prepare highly weather-resistant biodegradable plastic films by ejecting, granulating and blow molding processes.

Benefits of technology

It improves the anti-aging performance of biodegradable plastic film, solves the problems of uneven distribution of additives and migration, significantly improves the tensile strength and elongation of fracture of plastic film, and extends the service life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-weather-resistance biodegradable mulching film and a preparation method thereof. The raw materials comprise the following components in parts by mass: 100 parts of poly (terephthalic acid-butylene adipate) / polylactic acid, 1-7 parts of a high-weather-resistance auxiliary agent and 0.1-20 parts of other auxiliary agents; the preparation method comprises the following steps: (1) drying and mixing a hollow nanotube material and an anti-aging auxiliary agent, putting the mixture into a torque rheometer, carrying out a mixed reaction, and loading the anti-aging auxiliary agent on the hollow nanotube material in a chemical grafting and physical adsorption manner to obtain a reaction product; (2) mixing and reacting the reaction product with a coupling agent to obtain a high-weather-resistant auxiliary agent; the preparation method comprises the following steps: uniformly mixing the components, and sequentially extruding, granulating, drying and blow-molding the mixture to obtain the high-weather-resistance biodegradable mulching film. The prepared high-weather-resistance biodegradable mulching film has better anti-aging performance, and after aging is conducted for the same time, the tensile strength and the elongation at break are obviously superior to those of a biodegradable mulching film product prepared by physically mixing a hollow nano material and an anti-aging auxiliary.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of membrane materials, and in particular relates to a highly weather-resistant biodegradable ground membrane and a preparation method thereof. Background Art

[0003] Currently, biodegradable mulch is difficult to promote on a large scale and still faces many key technical challenges. A significant bottleneck is its poor weather resistance. Product performance rapidly declines with extended outdoor use, severely impacting its effective service life. While the addition of UV absorbers, antioxidants, and hydrolysis inhibitors to the formulation can improve the weather resistance of biodegradable mulch, due to limitations on the amount of small molecule additives that can be added to biodegradable materials, high concentrations of these additives often lead to uneven dispersion and migration within the biodegradable material, hindering the long-term weather resistance of products like biodegradable mulch. Summary of the Invention

[0004] The present invention aims to solve the key problem of poor weather resistance of current biodegradable mulch films and other products, and provides a highly weather-resistant biodegradable mulch film with a simple preparation method, high weather resistance and industrializability, and a preparation method thereof.

[0005] The highly weather-resistant biodegradable mulch film of the present invention is prepared by the following method:

[0006] The raw materials, calculated by weight, include: 100 parts of poly(butylene terephthalate-adipate) / polylactic acid, 1-7 parts of high weather resistance additives, and 0.1-20 parts of other additives;

[0007] The preparation method of the high weather resistance additive is as follows:

[0008] (1) The hollow nanotube material and the anti-aging agent are dried and mixed, and then placed in a torque rheometer for mixing reaction, and the hollow nanotube material is loaded with the anti-aging agent by chemical grafting and physical adsorption to obtain a reaction product;

[0009] (2) mixing the above reaction product with a coupling agent to obtain a high weathering resistant additive;

[0010] The various components are mixed uniformly, and the mixture is sequentially extruded, granulated, dried and blown to obtain a highly weather-resistant biodegradable ground film.

[0011] Preferably, the mass ratio of poly(butylene terephthalate-adipate) / polylactic acid is 99:1-70:30.

[0012] Preferably, the hollow nanotube material is one or both of halloysite nanotubes and carbon nanotubes.

[0013] Preferably, the anti-aging agent is one or more of benzophenone ultraviolet absorbers such as UV-531 and benzotriazole ultraviolet absorbers such as UV-360, antioxidants such as AT168 and AT1010, hindered amine light stabilizers such as bis-2,2,6,6-tetramethylpiperidinol sebacate, and anti-hydrolysis agents such as carbodiimide.

[0014] Preferably, the mass ratio of the hollow nanotube material to the anti-aging agent is 1:3-1:0.5.

[0015] Preferably, the reaction temperature in the torque rheometer is set to be 10-20° C. higher than the highest melting point of the anti-aging agent used, the reaction time is set to be 10-30 min, and the stirring speed is set to be 50-100 rpm.

[0016] Preferably, the coupling agent is one or both of a silane coupling agent such as 3-(2,3-epoxypropoxy)propyltrimethoxysilane and a titanate coupling agent such as tetraisopropyl bis(dioctylphosphite) titanate.

[0017] Preferably, the other additives include one or more of a chain extender, a dispersant, and an inorganic filler.

[0018] Preferably, the raw material components are calculated by weight as follows: 100 parts of poly (butylene terephthalate-adipate) / polylactic acid (mass ratio 9:1-8:2), 2-3 parts of high weather resistance additive, 0.4-0.5 parts of chain extender ADR-4468, 0.5-1 parts of silicone diffusion oil or epoxy soybean oil, and 10-15 parts of calcium carbonate;

[0019] Preparation method of high weathering resistant additive:

[0020] (1) 20 g of halloysite nanotubes, 3-4 g of ultraviolet absorber UV-P or UV-327, 1-1.5 g of hindered amine light stabilizer 770, 0.5-1 g of antioxidant AT1010, and 1.5 g of antioxidant AT168 were dried and mixed and then placed in a torque rheometer at a stirring speed of 80 rpm and a temperature of 145° C. for a mixing reaction for 25 min;

[0021] (2) 26 g of the above reaction product was mixed with 0.78 g of tetraisopropyl di(dioctylphosphite) titanate in a powder mixer to obtain a high weathering resistant additive;

[0022] Preparation process:

[0023] The above components were mixed in a high-speed mixer at 800 rpm for 10 min to obtain a uniformly mixed mixture; the mixture was sequentially extruded in a twin-screw extruder, and the temperatures of the processing sections of the twin-screw extruder were as follows: feeding section temperature 130-140°C, compression section temperature 140-160°C, homogenization temperature 145-175°C, homogenization temperature 145-175°C, and die temperature 150-180°C to obtain an extrudate; the extrudate was pelletized in a pelletizer at a rotation speed of 350 rpm. The extrudate particles are granulated to obtain extrudate particles with a particle size of 1.5-3 mm; the extrudate particles are dried in a drying kettle at 70° C. for 6 hours to make the moisture content of the extrudate particles lower than 0.05%, thereby obtaining dried extrudate particles; the extrudate particles are blow-molded in a film blowing machine, and the temperatures of the various processing sections of the blow molding are as follows: a feeding section temperature of 120-140° C., a compression section temperature of 130-150° C., a homogenization section temperature of 140-160° C., and a die temperature of 140-160° C., thereby obtaining a highly weather-resistant biodegradable mulch film.

[0024] The beneficial effects of the present invention are as follows:

[0025] (1) The high weathering-resistant additive prepared by the present invention, wherein the hollow nanotube material (such as halloysite nanotubes and carbon nanotubes) has a strong loading capacity, and can simultaneously quickly and efficiently fix the anti-aging additive by chemical grafting and physical adsorption. The obtained high weathering-resistant additive has a strong anti-aging function.

[0026] (2) The high weather resistance additive obtained by the present invention has good dispersibility, which can effectively solve the problems of uneven distribution of high-added anti-aging additives in biodegradable mulch, easy migration, and limited anti-aging effect.

[0027] (3) The method of preparing a highly weather-resistant additive of the present invention adopts a solid-phase reaction, which reduces the steps of filtering, washing, and drying in the conventional method of loading small molecules on nanomaterials. It is easy to operate, has a high yield, and has industrial prospects.

[0028] (4) The highly weather-resistant biodegradable mulch prepared by the present invention has better anti-aging performance. After the same aging time, the tensile strength and elongation at break are significantly better than those of the biodegradable mulch product prepared by physically mixing the hollow nanomaterials and the anti-aging additives. DETAILED DESCRIPTION

[0029] The following examples are provided to further illustrate the present invention, but are not intended to limit the present invention.

[0030] Example 1:

[0031] A highly weather-resistant biodegradable mulch film comprises the following raw materials in parts by weight: 100 parts of poly(butylene terephthalate-adipate) / polylactic acid (9:1), 2 parts of a highly weather-resistant additive, 0.4 parts of a chain extender ADR-4468, 0.5 parts of epoxy soybean oil, and 10 parts of calcium carbonate.

[0032] Preparation method of high weathering resistant additive:

[0033] (1) 20 g of halloysite nanotubes, 3 g of UV absorber UV-P, 1 g of hindered amine light stabilizer 770, 0.5 g of antioxidant AT1010, and 1.5 g of antioxidant AT168 were dried and mixed and then placed in a torque rheometer at a stirring speed of 80 rpm and a temperature of 145°C for a mixing reaction for 25 min;

[0034] (2) 26 g of the above reaction product and 0.78 g of tetraisopropyl di(dioctylphosphite) titanate were mixed and reacted in a powder mixer to obtain a high weathering resistance additive.

[0035] Preparation process:

[0036] All the above components were mixed in a high-speed mixer at 800 rpm for 10 minutes to obtain a uniformly mixed mixture; the mixture was sequentially extruded in a twin-screw extruder, and the temperatures of the processing sections of the twin-screw extruder were as follows: the feeding section temperature was 130-140°C, the compression section temperature was 140-160°C, the homogenization section temperature was 145-175°C, and the die temperature was 150-180°C to obtain an extrudate; the extrudate was granulated in a pelletizer at a speed of 350 rpm to obtain particles with a diameter of 1.5- 3mm extrudate particles; drying the extrudate particles in a drying kettle at 70°C for 6h to make the moisture content of the extrudate particles less than 0.05%, thereby obtaining dried extrudate particles; blow-molding the extrudate particles in a film blowing machine, wherein the temperatures of the various processing sections of the blow molding are: feeding section temperature 120-140°C, compression section temperature 130-150°C, homogenization section temperature 140-160°C, and die temperature 140-160°C, thereby obtaining a highly weather-resistant biodegradable mulch film with a thickness of 10μm.

[0037] Example 2:

[0038] A highly weather-resistant biodegradable mulch film, the main raw material components of which are, by weight, 100 parts of poly(butylene terephthalate-adipate) / polylactic acid (8:2), 3 parts of a high-weather-resistant additive, 0.5 parts of a chain extender ADR-4300, 1 part of an organosilicon diffusion oil, and 10 parts of calcium carbonate.

[0039] Preparation method of high weathering resistant additive:

[0040] (1) 20 g of halloysite nanotubes, 4 g of ultraviolet absorber UV-327, 1 g of hindered amine light stabilizer 622, 0.5 g of antioxidant AT1010, and 1.5 g of antioxidant AT168 were dried and mixed, and then placed in a torque rheometer at a stirring speed of 80 rpm and a temperature of 145° C. for a mixing reaction for 25 min to obtain a reaction product;

[0041] (2) The above reaction product was mixed with 0.81 g of tetraisopropyl di(dioctylphosphite) titanate in a powder mixer to obtain a high weathering resistance additive.

[0042] Preparation process:

[0043] All the above components were mixed in a high-speed mixer at 800 rpm for 10 minutes to obtain a uniformly mixed mixture; the mixture was sequentially extruded in a twin-screw extruder, and the temperatures of the processing sections of the twin-screw extruder were as follows: the feeding section temperature was 130-140°C, the compression section temperature was 140-160°C, the homogenization section temperature was 145-175°C, and the die temperature was 150-180°C to obtain an extrudate; the extrudate was granulated in a pelletizer at a speed of 350 rpm to obtain particles with a diameter of 1.5- 3mm extrudate particles; drying the extrudate particles in a drying kettle at 70°C for 6h to make the moisture content of the extrudate particles less than 0.05%, thereby obtaining dried extrudate particles; blow-molding the extrudate particles in a film blowing machine, wherein the temperatures of the various processing sections of the blow molding are: feeding section temperature 120-140°C, compression section temperature 130-150°C, homogenization section temperature 140-160°C, and die temperature 140-160°C, thereby obtaining a highly weather-resistant biodegradable mulch film with a thickness of 10μm.

[0044] Example 3:

[0045] A highly weather-resistant biodegradable mulch film, the main raw material components of which are, by weight, 100 parts of poly(butylene terephthalate-adipate) / polylactic acid (8:2), 3 parts of a high-weather-resistant additive, 0.5 parts of a chain extender ADR-4468, 1 part of epoxy soybean oil, and 15 parts of calcium carbonate.

[0046] Preparation method of high weathering resistant additive:

[0047] (1) 20 g of halloysite nanotubes, 3 g of ultraviolet absorber UV-327, 1.5 g of hindered amine light stabilizer 622, 1 g of antioxidant AT1010, and 1.5 g of antioxidant AT168 were dried and mixed, and then placed in a torque rheometer at a stirring speed of 80 rpm and a temperature of 145° C. for a mixing reaction for 25 min to obtain a reaction product;

[0048] (2) The above reaction product was mixed with 0.81 g of 3-(2,3-epoxypropoxy)propyltrimethoxysilane in a powder grinder to obtain a high weather resistance additive.

[0049] Preparation process:

[0050] All the above components were mixed in a high-speed mixer at 800 rpm for 10 minutes to obtain a uniformly mixed mixture; the mixture was sequentially extruded in a twin-screw extruder, and the temperatures of the processing sections of the twin-screw extruder were as follows: the feeding section temperature was 130-140°C, the compression section temperature was 140-160°C, the homogenization section temperature was 145-175°C, and the die temperature was 150-180°C to obtain an extrudate; the extrudate was granulated in a pelletizer at a speed of 350 rpm to obtain particles with a diameter of 1.5- 3mm extrudate particles; drying the extrudate particles in a drying kettle at 70°C for 6h to make the moisture content of the extrudate particles less than 0.05%, thereby obtaining dried extrudate particles; blow-molding the extrudate particles in a film blowing machine, wherein the temperatures of the various processing sections of the blow molding are: feeding section temperature 120-140°C, compression section temperature 130-150°C, homogenization section temperature 140-160°C, and die temperature 140-160°C, thereby obtaining a highly weather-resistant biodegradable mulch film with a thickness of 10μm.

[0051] Comparative Example 1:

[0052] Disclosed is an agricultural biodegradable mulch film, the main raw material components of which are, by weight, 100 parts of poly(butylene terephthalate-adipate) / polylactic acid (9:1), 2 parts of a weathering additive, 0.4 parts of a chain extender ADR-4468, 0.5 parts of epoxy soybean oil, and 10 parts of calcium carbonate.

[0053] Preparation method of weathering additive:

[0054] (1) 20 g of halloysite nanotubes, 3 g of ultraviolet absorber UV-P, 1 g of hindered amine light stabilizer 770, 0.5 g of antioxidant AT1010, and 1.5 g of antioxidant AT168 were dried and physically mixed in a high-speed mixer;

[0055] (2) Then, 0.78 g of tetraisopropyl di(dioctylphosphite) titanate was added to the high-pressure mixer and the mixture was continued to be mixed and stirred to obtain a weathering agent.

[0056] Preparation process:

[0057] All the above components were mixed in a high-speed mixer at 800 rpm for 10 min to obtain a uniformly mixed mixture; the mixture was sequentially extruded in a twin-screw extruder, and the temperatures of the processing sections of the twin-screw extruder were as follows: the feeding section temperature was 130-140°C, the compression section temperature was 140-160°C, the homogenization section temperature was 145-175°C, and the die temperature was 150-180°C to obtain an extrudate; the extrudate was granulated in a pelletizer at a speed of 350 rpm to obtain a particle size of 1.5 -3mm extrudate particles; drying the extrudate particles in a drying kettle at 70°C for 6 hours to make the moisture content of the extrudate particles less than 0.05%, thereby obtaining dried extrudate particles; blow-molding the extrudate particles in a film blowing machine, wherein the temperatures of the various processing sections of the blow molding are: a feeding section temperature of 120-140°C, a compression section temperature of 130-150°C, a homogenization section temperature of 140-160°C, and a die temperature of 140-160°C, thereby obtaining an agricultural biodegradable mulch film with a thickness of 10 μm.

[0058] The performance tests were conducted on the mulch films of Examples 1, 2, and 3 and the mulch film of Comparative Example 1. The test standards were as follows: tensile strength and elongation at break were tested according to GB\T1040.3-2006, and UV aging was tested according to GB\T16422-2006. The test results are shown in Table 1.

[0059] Table 1

[0060] performance Example 1 Example 2 Example 3 Comparative Example 1 Tensile strength MPa 25 27 30 25 Elongation at break % 410 522 520 450 UV aging 100h, elongation at break retention rate, % 70 81 77 33

Claims

1. A method for preparing a highly weather-resistant biodegradable mulch film, characterized in that: The following steps are involved: The raw materials, by weight, include: 100 parts of poly(butylene terephthalate-adipate) / polylactic acid, 1-7 parts of high weather resistance additives, and 0.1-20 parts of other additives; The high weather resistance additive is prepared by: (1) The hollow nanotube material and the anti-aging agent are dried and mixed, and then placed in a torque rheometer for mixing reaction, and the hollow nanotube material is loaded with the anti-aging agent by chemical grafting and physical adsorption to obtain a reaction product; (2) mixing the above reaction product with a coupling agent to obtain a high weathering resistant additive; The components are mixed uniformly, and the mixture is sequentially extruded, granulated, dried and blow-molded to obtain a highly weather-resistant biodegradable mulch film.

2. The preparation method according to claim 1, characterized in that: The mass ratio of poly(butylene terephthalate-adipate) / polylactic acid is 99:1-70:

30.

3. The preparation method according to claim 1, characterized in that: The hollow nanotube material is one or both of halloysite nanotubes and carbon nanotubes.

4. The preparation method according to claim 1, characterized in that: The anti-aging aid is one or more of benzophenone ultraviolet absorbers such as UV-531 and benzotriazole ultraviolet absorbers such as UV-360, antioxidants such as AT168 and AT1010, hindered amine light stabilizers such as bis-2,2,6,6-tetramethylpiperidinol sebacate, and anti-hydrolysis agents such as carbodiimide.

5. The preparation method according to claim 1, characterized in that: The mass ratio of the hollow nanotube material to the anti-aging additive is 1:3-1:0.

5.

6. The preparation method according to claim 1, characterized in that: The reaction temperature in the torque rheometer is set to be 10-20° C. higher than the highest melting point of the anti-aging agent used, the reaction time is set to be 10-30 min, and the stirring speed is set to be 50-100 rpm.

7. The preparation method according to claim 1, characterized in that: The coupling agent is one or two of silane coupling agents such as 3-(2,3-epoxypropoxy)propyltrimethoxysilane and the like, and titanate coupling agents such as tetraisopropyl di(dioctylphosphite) titanate and the like.

8. The preparation method according to claim 1, characterized in that: The other auxiliary agents include one or more of a chain extender, a dispersant, and an inorganic filler.

9. The preparation method according to claim 1, characterized in that: The raw material components are calculated by weight: including: 100 parts of poly (butylene terephthalate-adipate) / polylactic acid (mass ratio 9:1-8:2), 2-3 parts of high weather resistance additive, 0.4-0.5 parts of chain extender ADR-4468, 0.5-1 parts of silicone diffusion oil or epoxy soybean oil, and 10-15 parts of calcium carbonate; Preparation method of high weathering resistant additive: (1) 20 g of halloysite nanotubes, 3-4 g of ultraviolet absorber UV-P or UV-327, 1-1.5 g of hindered amine light stabilizer 770, 0.5-1 g of antioxidant AT1010, and 1.5 g of antioxidant AT168 were dried and mixed, and then placed in a torque rheometer, stirred at a speed of 80 rpm and a temperature of 145° C. for a mixing reaction for 25 min; (2) 26 g of the above reaction product was mixed with 0.78 g of tetraisopropyl di(dioctylphosphite) titanate in a powder mill to obtain a high weathering resistant additive; Preparation process: The above components were mixed in a high-speed mixer at 800 rpm for 10 minutes to obtain a uniformly mixed mixture; the mixture was sequentially extruded in a twin-screw extruder, and the temperatures of the processing sections of the twin-screw extruder were: a feeding section temperature of 130-140°C, a compression section temperature of 140-160°C, a homogenization temperature of 145-175°C, a homogenization temperature of 145-175°C, and a die temperature of 150-180°C to obtain an extrudate; the extrudate was pelletized in a pelletizer at a rotation speed of 350 rpm. The extrusion material particles are obtained by drying the extrusion material particles in a drying kettle at 70°C for 6 hours to make the moisture content of the extrusion material particles lower than 0.05%, thereby obtaining dried extrusion material particles; the extrusion material particles are blow-molded in a film blowing machine, and the temperatures of the various processing sections of the blow molding are as follows: the feeding section temperature is 120-140°C, the compression section temperature is 130-150°C, the homogenization section temperature is 140-160°C, and the die temperature is 140-160°C, thereby obtaining a highly weather-resistant biodegradable mulch film.

Citation Information

Cited By

  • Anti-aging master batch for producing full-biodegradable mulching film and preparation method of anti-aging master batch

    CN120590762A

  • Composite degradation accelerant, controllable degradation biological material and preparation method of controllable degradation biological material