Two-component polyurethane coating for decorative plate and preparation method of two-component polyurethane coating

By introducing fluorine element and POSS structure into decorative panel coatings, combining hydrophobic and flame retardant, and using hyperbranched polyol chain extension technology, the limitations of traditional coatings in terms of impact resistance, hydrophobic and flame retardant are solved, and the limitations of traditional coatings are achieved. High-performance two-component polyurethane coating improves the overall performance of decorative panels.

CN118956256AInactive Publication Date: 2024-11-15TAIZHOU BAIDAI DECORATION MATERIAL CO LTD

Patent Information

Application Number
CN202411196906.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional decorative panel coatings show limitations in impact resistance, hydrophobicity, flame retardancy and adhesion, and cannot meet the high requirements of modern buildings for multifunctional performance.

Method used

Using two-component polyurethane coating, the coating with excellent mechanical properties, hydrophobic properties and flame retardant properties is prepared by introducing fluorine elements and POSS structures, combining hydrophobic additives and flame retardant agents, and the coating with excellent mechanical properties, hydrophobic properties and flame retardant properties are improved through hyperbranched polyol chain extension technology. Focus and disperse performance.

Benefits of technology

It significantly improves the impact resistance, hydrophobicity and flame retardant properties of the coating, extends the service life of decorative sheets, and expands its application scenarios, avoids the dispersion problem of additional individual additives, and improves the stability of the resin. and hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005016717540000111
    Figure BDA0005016717540000111
Patent Text Reader

Abstract

The invention discloses a bi-component polyurethane coating for a decorative plate and a preparation method of the bi-component polyurethane coating, and relates to the technical field of polyurethane, the preparation method of the bi-component polyurethane coating comprises the following steps: uniformly mixing POSS hybrid polyurethane acrylate, hyperbranched polyurethane acrylate, an active diluent, pentaerythritol triacrylate and a photoinitiator 1173 according to a ratio, adding a curing agent, and uniformly stirring to obtain the bi-component polyurethane coating for the decorative plate. The two-component polyurethane coating is obtained; the double-component polyurethane coating is prepared from the following components in parts by mass: 10 to 25 parts of POSS (Polyhedral Oligomeric Silsesquioxane) hybrid polyurethane acrylate, 35 to 60 parts of hyperbranched polyurethane acrylate, 5 to 10 parts of reactive diluent, 20 to 25 parts of pentaerythritol triacrylate and 3 to 6 parts of photoinitiator 1173.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane, in particular to a two-component polyurethane coating for decorative plates and a preparation method thereof. Background Art

[0002] With the development of building decoration materials, the requirements for decorative panels are getting higher and higher. Modern buildings not only pursue beauty, but also require materials to have multifunctional properties, such as impact resistance, hydrophobicity, flame retardancy and adhesion. Traditional decorative panels usually use single-component coatings. Although these coatings are easy to apply, they have certain limitations in terms of impact resistance, hydrophobicity, flame retardancy and adhesion to the substrate, and cannot meet high-demand application scenarios. Two-component polyurethane coatings can significantly improve performance due to their unique chemical structure and cross-linking reaction.

[0003] Its high cross-linking density can give the coating excellent mechanical properties, including better impact resistance, significantly improving the damage resistance of decorative panels. In addition, polyurethane coatings can significantly enhance the waterproof and anti-fouling capabilities of the coating by introducing special hydrophobic additives. By adding flame retardants, two-component polyurethane coatings can also improve the flame retardant properties of decorative panels, thereby enhancing their safety in public places. Strong adhesion ensures that the coating forms a firm bond on the surface of various substrates, extending the service life of decorative panels.

[0004] Therefore, developing a two-component polyurethane coating with excellent impact resistance, hydrophobicity, flame retardancy and adhesion properties is of great significance for improving the comprehensive performance of decorative panels. Summary of the invention

[0005] The object of the present invention is to provide a two-component polyurethane coating for decorative panels and a preparation method thereof, so as to solve the problems raised in the prior art.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a two-component polyurethane coating for decorative panels, characterized in that: S1: adding lithium hydroxide and deionized water to tetrahydrofuran, stirring at room temperature for 10-15 minutes, adding phenyltriethoxysilane, controlling the dropping time, heating to 38-40° C. to react for 24-36 hours, and post-treating to obtain trisilanol POSS;

[0008] Furthermore, the dripping time is controlled to be 1-2h;

[0009] Furthermore, the post-treatment process includes the following steps: vacuum degree of 0.1MPa, temperature of 40°C, rotary evaporation to remove solvent, adding methanol to dissolve, filtering, collecting supernatant, adding the supernatant to 10wt% sodium chloride solution under stirring, filtering, washing precipitate with deionized water, adding chloroform to dissolve, filtering, collecting supernatant, vacuum degree of 0.1MPa, temperature of 40°C, rotary evaporation to remove solvent, vacuum drying for 12h;

[0010] Further, in the trisilanol POSS, the molar ratio of phenyltriethoxysilane: lithium hydroxide: deionized water is 1: 0.44: 1.5;

[0011] S2: Add butyl-decanoic acid, terephthalic acid methanol, and diphenyl phosphate into a reaction container, stir at room temperature for 12-14 hours, add acetone to dissolve, wash with 1 mg / mL potassium hydroxide solution, filter, collect the oil phase, add ethyl acetate to dissolve, wash with deionized water, filter, collect the oil phase, and dry by rotary evaporation to remove the solvent to obtain polydecanoic acid diol A;

[0012] Furthermore, in the polydecanolide diol A, the molar ratio of butyl-decanolide: terephthalic acid alcohol: diphenyl phosphate is (20-40): (5-10): (1-2);

[0013] S3: Add 1,4-o-phthalaldehyde and ethanolamine to anhydrous ethanol, stir evenly, heat to 85-90°C for reaction for 5-5.5h, add DOPO, keep warm and continue to react for 12h, cool to room temperature, filter, remove the solvent by rotary evaporation, wash with ethanol, and vacuum dry at 60°C for 24h to obtain flame retardant modified diol;

[0014] Furthermore, in the flame retardant modified diol, the molar ratio of 1,4-o-phthalaldehyde:ethanolamine:DOPO is (1-2):(2-4):(2-4);

[0015] S4: Add butyl decanolactone, flame retardant modified diol, and diphenyl phosphate into a reaction container, stir at room temperature for 12-14 hours, add acetone to dissolve, wash with 1 mg / mL potassium hydroxide solution, filter, collect the oil phase, add ethyl acetate to dissolve, wash with deionized water, filter, collect the oil phase, and dry by rotary evaporation to remove the solvent to obtain polydecanolactone diol B;

[0016] Furthermore, in the polydecanolide diol B, the molar ratio of butyl-decanolide: flame retardant modified diol: diphenyl phosphate is (20-40): (4-12): (1-2);

[0017] S5: adding isophorone diisocyanate to a reaction vessel, preheating to 65°C under a nitrogen atmosphere, adding tetrafluoropropanol and dibutyltin dilaurate, heating to 90-91°C for reaction for 2-3h, adding trihydroxypropane, and keeping the temperature to react until the isocyanate group content in the system reaches the theoretical value, thereby obtaining a fluorinated diol;

[0018] Furthermore, in the fluorinated diol, the molar ratio of isophorone diisocyanate:tetrafluoropropanol:trihydroxypropane is 1:1:1;

[0019] S6: Add polydecanoic acid diol A and isophorone diisocyanate to a reaction container, stir evenly, add a reactive diluent to dilute the reaction system into a solution, heat to 65-66°C for reaction for 2h, add fluorinated diol and dibutyltin dilaurate, heat to 90-91°C for reaction for 2-3h, add trisilanol POSS, add a reactive diluent to dilute the reaction system into a solution, cool to 70-71°C for reaction for 3-3.5h, add hydroxypropyl acrylate, heat to 78°C for reaction for 4-5h, and obtain POSS hybrid polyurethane acrylate;

[0020] Further, the proportion of each component in the POSS hybrid polyurethane acrylate includes, by mass, 4-8 parts of polydecanoic acid diol A, 6-12 parts of isophorone diisocyanate, 0.5-1 parts of reactive diluent, 6-12 parts of fluorinated diol, 0.6-1.2 parts of trisilanol POSS, 4-8 parts of hydroxypropyl acrylate, and 0.02-0.03 parts of dibutyltin dilaurate;

[0021] Further, the active diluent is 1,6-hexanediol diacrylate;

[0022] S7: Add polydecanoic acid diol B to a reaction container, stir evenly, preheat to 60°C, add isophorone diisocyanate and dibutyltin dilaurate, heat to 80-81°C for reaction for 1-1.5h, cool to 70°C, add hydroxyethyl acrylate and keep warm for reaction for 2-2.5h, add pentaerythritol triacrylate, heat to 84-85°C for reaction for 2-2.5h, add hyperbranched polyol, keep warm for reaction until the isocyanate group content in the system reaches the theoretical value, and obtain hyperbranched polyurethane acrylate;

[0023] Furthermore, the proportions of the components in the hyperbranched polyurethane acrylate include, by mass, 4-8 parts of polydecanoic acid diol B, 5-10 parts of isophorone diisocyanate, 1.2-2.4 parts of hydroxyethyl acrylate, 1.3-2.6 parts of pentaerythritol triacrylate, 0.5-1.0 parts of hyperbranched polyol, and 0.02-0.03 parts of dibutyltin dilaurate;

[0024] S8: POSS hybrid polyurethane acrylate, hyperbranched polyurethane acrylate, reactive diluent, pentaerythritol triacrylate and photoinitiator 1173 are uniformly mixed in proportion to obtain a two-component polyurethane coating.

[0025] Furthermore, the proportions of the components in the two-component polyurethane coating, by mass, include: 10-25 parts of POSS hybrid polyurethane acrylate, 35-60 parts of hyperbranched polyurethane acrylate, 5-10 parts of active diluent, 20-25 parts of pentaerythritol triacrylate, and 11733-6 parts of photoinitiator.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The invention uses butyl-decanolide, terephthalic acid methanol, diphenyl phosphate and butyl-decanolide, flame-retardant modified diol and diphenyl phosphate as raw materials to prepare polydecanolide diol A containing hydrophobic side chains and polydecanolide diol B containing hydrophobic and flame-retardant side chains; then, using polydecanolide diol A as raw material, fluorine element is uniformly introduced into polyurethane acrylate molecular chain segments by chain extension of fluorinated diol; in the same chain extension method, using trisilanol POSS as chain extender, POSS structure is uniformly introduced into polyurethane acrylate molecular chain segments; on the one hand, the introduction of fluorine element and POSS structure can give coating excellent hydrophobic property, avoid additional reinforcing auxiliary agent added separately, solve the problem of dispersibility of traditional fluorine-containing small molecules and POSS in polyurethane acrylate, and greatly improve the stability of resin; on the other hand, the introduction of POSS can greatly enhance the hardness of coating, improve impact resistance and wear resistance at the same time, prolong the service life of decorative plate and expand the application scene of decorative plate.

[0028] In order to further improve the adhesion and flame retardant properties of two-component polyurethane coatings and expand the application scenarios of decorative plates, the present invention plans to introduce another polyurethane acrylate (hyperbranched polyurethane acrylate) to achieve the purpose of improving the dispersion performance of POSS hybrid polyurethane acrylate, adjusting the viscosity of two-component polyurethane coatings, improving the adhesion of two-component polyurethane coatings, and imparting flame retardant properties to two-component polyurethane coatings. The flame retardant modified diol is a small molecule diol, and a hyperbranched polyol is introduced into a molecular segment by chain extension, while maintaining the excellent mechanical properties and hydrophobic properties of the two-component polyurethane coating, the dispersion performance of POSS hybrid polyurethane acrylate is improved, the viscosity of the two-component polyurethane coating is adjusted, multiple carbon-carbon double bonds are introduced to improve the adhesion of the two-component polyurethane coating, and the DOPO structure in the segment imparts flame retardant properties to the two-component polyurethane coating, and finally a two-component polyurethane coating with excellent mechanical properties, hydrophobic properties and flame retardant properties is prepared. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the following examples, the hyperbranched polyol model is Boltorn TM H2004, M n =3200, purchased from Guangzhou Haoyi New Material Technology Co., Ltd.; the rest were originally commercially available.

[0031] In the following embodiment, the preparation method of trisilanol POSS comprises the following steps: 0.44 mol lithium hydroxide and 1.5 mol deionized water are added to 250 mL tetrahydrofuran, stirred at room temperature for 10 min, 1 mol phenyltriethoxysilane is added dropwise within 1 h, heated to 38 ° C for reaction for 24 h, vacuum degree is 0.1 MPa, the temperature is 40 ° C, the solvent is removed by rotary evaporation, methanol is added to dissolve, filtered, the supernatant is collected, the supernatant is added to 10 wt % sodium chloride solution under stirring, filtered, the precipitate is washed with deionized water, chloroform is added to dissolve, filtered, the supernatant is collected, the vacuum degree is 0.1 MPa, the temperature is 40 ° C, the solvent is removed by rotary evaporation, and vacuum drying is 12 h to obtain trisilanol POSS.

[0032] The preparation method of flame retardant modified diol comprises the following steps: adding 1 mol 1,4-o-phthalaldehyde and 2 mol ethanolamine into anhydrous ethanol, stirring evenly, heating to 85°C for reaction for 5 hours, adding 2 mol DOPO, keeping warm and continuing the reaction for 12 hours, cooling to room temperature, filtering, rotary evaporation to remove the solvent, washing with ethanol, and vacuum drying at 60°C for 24 hours to obtain flame retardant modified diol.

[0033] The preparation method of fluorinated diol comprises the following steps: adding 1 mol of isophorone diisocyanate into a reaction container, preheating to 65°C under a nitrogen atmosphere, adding 1 mol of tetrafluoropropanol and 0.02 mol of dibutyltin dilaurate, heating to 90°C for reaction for 2 hours, adding 1 mol of trihydroxypropane, and keeping the temperature to react until the isocyanate group content in the system reaches a theoretical value, thereby obtaining fluorinated diol.

[0034] The preparation method of polydecanolactone diol A comprises the following steps: adding 20 mol of butyl-decanoic acid, 5 mol of terephthalic acid methanol and 1 mol of diphenyl phosphate into a reaction container, stirring at room temperature for 12 hours, adding acetone to dissolve, washing with 1 mg / mL potassium hydroxide solution, filtering, collecting an oil phase, adding ethyl acetate to dissolve, washing with deionized water, filtering, collecting an oil phase, and rotary drying to remove the solvent to obtain polydecanolactone diol A.

[0035] The preparation method of polydecanolactone diol B comprises the following steps: adding 20 mol of butyl-decanoic acid, 8 mol of flame-retardant modified diol and 1 mol of diphenyl phosphate into a reaction container, stirring at room temperature for 12 hours, adding acetone to dissolve, washing with 1 mg / mL potassium hydroxide solution, filtering, collecting oil phase, adding ethyl acetate to dissolve, washing with deionized water, filtering, collecting oil phase, and rotary drying to remove the solvent to obtain polydecanolactone diol B.

[0036] Embodiment 1: A method for preparing a two-component polyurethane coating for decorative panels: S1: Add 4 parts of polydecanoic acid diol A and 6 parts of isophorone diisocyanate into a reaction container, stir evenly, add 0.2 parts of active diluent to dilute the reaction system into a solution, heat to 65°C for reaction for 2h, add 6 parts of fluorinated diol and 0.02 parts of dibutyltin dilaurate, heat to 90°C for reaction for 2h, add 0.6 parts of trisilanol POSS, add 0.3 parts of active diluent to dilute the reaction system into a solution, cool to 70°C for reaction for 3h, add 4 parts of hydroxypropyl acrylate, heat to 78°C for reaction for 4h, and obtain POSS hybrid polyurethane acrylate;

[0037] S2: Add 4 g of polydecanoic acid diol B to a reaction container, stir evenly, preheat to 60°C, add 5 g of isophorone diisocyanate and 0.02 g of dibutyltin dilaurate, heat to 80°C for reaction for 1 h, cool to 70°C, add 1.2 g of hydroxyethyl acrylate and keep warm for reaction for 2 h, add 1.3 g of pentaerythritol triacrylate, heat to 84°C for reaction for 2 h, add 0.5 g of hyperbranched polyol, keep warm for reaction until the isocyanate group content in the system reaches the theoretical value, and obtain hyperbranched polyurethane acrylate;

[0038] S3: 10 g of POSS hybrid polyurethane acrylate, 60 g of hyperbranched polyurethane acrylate, 5 g of reactive diluent, 20 g of pentaerythritol triacrylate, and 3 g of photoinitiator 1173 were mixed uniformly in proportion to obtain a two-component polyurethane coating.

[0039] Example 2: A method for preparing a two-component polyurethane coating for decorative panels: S1: Add 4 parts of polydecanoic acid diol A and 6 parts of isophorone diisocyanate into a reaction container, stir evenly, add 0.2 parts of active diluent to dilute the reaction system into a solution, heat to 65°C for reaction for 2h, add 8 parts of fluorinated diol and 0.02 parts of dibutyltin dilaurate, heat to 90°C for reaction for 2h, add 1 part of trisilanol POSS, add 0.3 parts of active diluent to dilute the reaction system into a solution, cool to 70°C for reaction for 3h, add 4 parts of hydroxypropyl acrylate, heat to 78°C for reaction for 4h, and obtain POSS hybrid polyurethane acrylate;

[0040] The remaining steps are the same as those in Example 1.

[0041] Example 3: A method for preparing a two-component polyurethane coating for decorative panels: S2: Add 8g of polydecanoic acid diol B into a reaction container, stir evenly, preheat to 60°C, add 5g of isophorone diisocyanate and 0.02g of dibutyltin dilaurate, heat to 80°C for reaction for 1h, cool to 70°C, add 1.2g of hydroxyethyl acrylate and keep warm for reaction for 2h, add 1.3g of pentaerythritol triacrylate, heat to 84°C for reaction for 2h, add 0.5g of hyperbranched polyol, keep warm for reaction until the isocyanate group content in the system reaches the theoretical value, and obtain hyperbranched polyurethane acrylate;

[0042] The remaining steps are the same as those in Example 1.

[0043] Example 4: A method for preparing a two-component polyurethane coating for decorative panels: S3: 20g POSS hybrid polyurethane acrylate, 50g hyperbranched polyurethane acrylate, 5g active diluent, 20g pentaerythritol triacrylate, and 3g photoinitiator 1173 are mixed uniformly in proportion to obtain a two-component polyurethane coating.

[0044] The remaining steps are the same as those in Example 1.

[0045] Comparative Example 1: A method for preparing a two-component polyurethane coating for decorative panels: S1: Add 4 parts of polydecanoic acid diol A and 6 parts of isophorone diisocyanate into a reaction container, stir evenly, add 0.2 parts of active diluent to dilute the reaction system into a solution, heat to 90°C for reaction for 2h, add 0.6 parts of trisilanol POSS and 0.02 parts of dibutyltin dilaurate, add 0.3 parts of active diluent to dilute the reaction system into a solution, cool to 70°C for reaction for 3h, add 4 parts of hydroxypropyl acrylate, heat to 78°C for reaction for 4h, and obtain POSS hybrid polyurethane acrylate;

[0046] S2: Add 4 g of polydecanoic acid diol B to a reaction container, stir evenly, preheat to 60°C, add 5 g of isophorone diisocyanate and 0.02 g of dibutyltin dilaurate, heat to 80°C for reaction for 1 h, cool to 70°C, add 1.2 g of hydroxyethyl acrylate and keep warm for reaction for 2 h, add 1.3 g of pentaerythritol triacrylate, heat to 84°C for reaction for 2 h, add 0.5 g of hyperbranched polyol, keep warm for reaction until the isocyanate group content in the system reaches the theoretical value, and obtain hyperbranched polyurethane acrylate;

[0047] S3: 10 g POSS hybrid polyurethane acrylate, 60 g hyperbranched polyurethane acrylate, 5 g reactive diluent, 20 g pentaerythritol triacrylate, 5 g hexafluorodecyl methacrylate, and 3 g photoinitiator 1173 were mixed uniformly in proportion to obtain a two-component polyurethane coating.

[0048] Comparative Example 2: A method for preparing a two-component polyurethane coating for decorative panels: 20 mol of butyl decanolactone, 8 mol of 1,4-butanediol, and 1 mol of diphenyl phosphate were added to a reaction container, stirred at room temperature for 12 hours, added with acetone to dissolve, washed with 1 mg / mL potassium hydroxide solution, filtered, the oil phase was collected, added with ethyl acetate to dissolve, washed with deionized water, filtered, the oil phase was collected, and the solvent was removed by rotary evaporation to obtain polydecanolactone diol B;

[0049] S3: 10 g POSS hybrid polyurethane acrylate, 60 g hyperbranched polyurethane acrylate, 5 g DOPO, 5 g active diluent, 20 g pentaerythritol triacrylate, and 3 g photoinitiator 1173 were mixed uniformly in proportion to obtain a two-component polyurethane coating.

[0050] The remaining steps are the same as those in Example 1.

[0051] Comparative Example 3: A method for preparing a two-component polyurethane coating for decorative panels: S2: Add 4 g of polydecanoic acid diol B into a reaction container, stir evenly, preheat to 60°C, add 5 g of isophorone diisocyanate and 0.02 g of dibutyltin dilaurate, heat to 80°C for reaction for 1 h, cool to 70°C, add 1.2 g of hydroxyethyl acrylate and keep warm for reaction for 2 h, add 2.1 g of pentaerythritol triacrylate, keep warm for reaction until the isocyanate group content in the system reaches the theoretical value, and obtain hyperbranched polyurethane acrylate;

[0052] The remaining steps are the same as those in Example 1.

[0053] Comparative Example 4: A method for preparing a two-component polyurethane coating for decorative panels: S3: 30 g of POSS hybrid polyurethane acrylate, 40 g of hyperbranched polyurethane acrylate, 5 g of reactive diluent, 20 g of pentaerythritol triacrylate, and 3 g of photoinitiator 1173 were uniformly mixed in proportion to obtain a two-component polyurethane coating;

[0054] The remaining steps are the same as those in Example 1.

[0055] Comparative Example 5: A method for preparing a two-component polyurethane coating for decorative panels: S3: 5 g of POSS hybrid polyurethane acrylate, 65 g of hyperbranched polyurethane acrylate, 5 g of active diluent, 20 g of pentaerythritol triacrylate, and 3 g of photoinitiator 1173 were mixed uniformly in proportion to obtain a two-component polyurethane coating;

[0056] The remaining steps are the same as those in Example 1.

[0057] Experiment: After removing bubbles from the two-component polyurethane coating prepared in the above examples and comparative examples, the coating was evenly coated on the surface of the decorative plate, placed in a UV curing machine for 5 minutes, and UV-cured to obtain a coating sample to be tested.

[0058] Adhesion test: Tested with a paint film cross-cut tester in accordance with GB / T 1720-1979.

[0059] Impact resistance test: The impact resistance of the coating was tested using an impact tester according to ASTM D2794-93 (2019).

[0060] Contact angle test: The water contact angle of the cured coating was tested using a DSA20 contact angle meter, with a micro syringe dripping at 25°C.

[0061] The two-component polyurethane coating prepared in the above examples and comparative examples was poured into a polytetrafluoroethylene mold after removing bubbles, placed in a UV curing machine for 24 hours, and UV-cured to obtain a cured film to be tested. The size of the cured film was 100 mm×10 mm×3 mm.

[0062] Limiting Oxygen Index Test: Tested according to test method ASTM D2863-2009.

[0063] Vertical burning test: The test is conducted in accordance with the national standard GB / T 2408-2008.

[0064] The experimental data are described in Table 1 below.

[0065] Table 1 Two-component polyurethane coating performance test data table

[0066]

[0067] Conclusion: The two-component polyurethane coating prepared by the present invention has excellent mechanical properties, hydrophobic properties and flame retardant properties.

[0068] Comparative Example 1: No fluorinated diol was added during the preparation of POSS hybrid polyurethane acrylate, and a fluorinated small molecule (hexafluorodecyl methacrylate) was added alone during the preparation of the two-component polyurethane coating, resulting in reduced dispersibility and stability of the two-component polyurethane coating, and reduced mechanical and hydrophobic coating properties of the two-component polyurethane;

[0069] In Comparative Example 2, no flame retardant modified diol was added during the preparation of polydecanoic acid diol B, and a flame retardant component (DOPO) was added alone during the preparation of the two-component polyurethane coating, resulting in reduced dispersibility of the two-component polyurethane coating and reduced flame retardant properties of the two-component polyurethane coating;

[0070] In the process of preparing the hyperbranched polyurethane acrylate in Comparative Example 3, no hyperbranched polyol was added for chain extension, resulting in an increase in viscosity and a decrease in stability of the prepared two-component polyurethane coating, an increase in entanglement between molecular chains, a decrease in toughness, and a decrease in mechanical properties of the two-component polyurethane coating;

[0071] In Comparative Example 4, too much POSS hybrid polyurethane acrylate was added during the preparation of the two-component polyurethane coating, and there was a lack of sufficient hyperbranched polyurethane acrylate to improve the dispersibility of the POSS hybrid polyurethane acrylate, resulting in reduced performance of the two-component polyurethane coating.

[0072] In comparative example 5, too much hyperbranched polyurethane acrylate was added during the preparation of the two-component polyurethane coating. The increased degree of hyperbranching resulted in increased difficulty in the polymerization reaction, which led to reduced performance of the two-component polyurethane coating.

[0073] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing a two-component polyurethane coating for decorative panels, characterized in that: S1: Add polydecanoic acid diol A and isophorone diisocyanate to a reaction container, stir evenly, add a reactive diluent to dilute the reaction system into a solution, heat to 65-66°C for reaction for 2h, add fluorinated diol and dibutyltin dilaurate, heat to 90-91°C for reaction for 2-3h, add trisilanol POSS, add a reactive diluent to dilute the reaction system into a solution, cool to 70-71°C for reaction for 3-3.5h, add hydroxypropyl acrylate, heat to 78°C for reaction for 4-5h, and obtain POSS hybrid polyurethane acrylate; S2: Add polydecanoic acid diol B to a reaction container, stir evenly, preheat to 60°C, add isophorone diisocyanate and dibutyltin dilaurate, heat to 80-81°C for reaction for 1-1.5h, cool to 70°C, add hydroxyethyl acrylate and keep warm for reaction for 2-2.5h, add pentaerythritol triacrylate, heat to 84-85°C for reaction for 2-2.5h, add hyperbranched polyol, keep warm for reaction until the isocyanate group content in the system reaches the theoretical value, and obtain hyperbranched polyurethane acrylate; S3: POSS hybrid polyurethane acrylate, hyperbranched polyurethane acrylate, reactive diluent, pentaerythritol triacrylate and photoinitiator 1173 are uniformly mixed in proportion to obtain a two-component polyurethane coating.

2. The method for preparing a two-component polyurethane coating for decorative panels according to claim 1, characterized in that: The proportions of the components in the POSS hybrid polyurethane acrylate include, by mass, 4-8 parts of polydecanoic acid diol A, 6-12 parts of isophorone diisocyanate, 0.5-1 parts of reactive diluent, 6-12 parts of fluorinated diol, 0.6-1.2 parts of trisilanol POSS, 4-8 parts of hydroxypropyl acrylate, and 0.02-0.03 parts of dibutyltin dilaurate.

3. The method for preparing a two-component polyurethane coating for decorative panels according to claim 1, characterized in that: The proportions of the components in the hyperbranched polyurethane acrylate include, by mass, 4-8 parts of polydecanoic acid diol B, 5-10 parts of isophorone diisocyanate, 1.2-2.4 parts of hydroxyethyl acrylate, 1.3-2.6 parts of pentaerythritol triacrylate, 0.5-1.0 parts of hyperbranched polyol, and 0.02-0.03 parts of dibutyltin dilaurate.

4. The method for preparing a two-component polyurethane coating for decorative panels according to claim 1, characterized in that: The proportions of the components in the two-component polyurethane coating, by weight, include: 10-25 parts of POSS hybrid polyurethane acrylate, 35-60 parts of hyperbranched polyurethane acrylate, 5-10 parts of active diluent, 20-25 parts of pentaerythritol triacrylate, and 11733-6 parts of photoinitiator.

5. The method for preparing a two-component polyurethane coating for decorative panels according to claim 1, characterized in that: The preparation method of polydecanolactone diol A comprises the following steps: adding butyl-decanolactone, terephthalic acid methanol and diphenyl phosphate into a reaction container, stirring at room temperature for 12-14 hours, adding acetone to dissolve, washing with 1 mg / mL potassium hydroxide solution, filtering, collecting the oil phase, adding ethyl acetate to dissolve, washing with deionized water, filtering, collecting the oil phase, and rotary drying to remove the solvent to obtain polydecanolactone diol A; In the polydecanolide diol A, the molar ratio of butyl-decanolide: terephthalic acid methanol: diphenyl phosphate is (20-40): (5-10): (1-2).

6. The method for preparing a two-component polyurethane coating for decorative panels according to claim 1, characterized in that: The preparation method of polydecanolactone diol B comprises the following steps: adding butyl-decanolactone, flame-retardant modified diol and diphenyl phosphate into a reaction container, stirring at room temperature for 12-14 hours, adding acetone to dissolve, washing with 1 mg / mL potassium hydroxide solution, filtering, collecting oil phase, adding ethyl acetate to dissolve, washing with deionized water, filtering, collecting oil phase, and rotary drying to remove solvent to obtain polydecanolactone diol B; In the polydecanolide diol B, the molar ratio of butyl-decanolide: flame retardant modified diol: diphenyl phosphate is (20-40): (4-12): (1-2).

7. The method for preparing a two-component polyurethane coating for decorative panels according to claim 6, characterized in that: The preparation method of the flame retardant modified diol, The method comprises the following steps: adding 1,4-o-phthalaldehyde and ethanolamine to anhydrous ethanol, stirring evenly, heating to 85-90°C for reaction for 5-5.5 hours, adding DOPO, keeping the temperature to continue the reaction for 12 hours, cooling to room temperature, filtering, removing the solvent by rotary evaporation, washing with ethanol, and vacuum drying at 60°C for 24 hours to obtain a flame retardant modified diol; In the flame retardant modified diol, the molar ratio of 1,4-o-phthalaldehyde:ethanolamine:DOPO is (1-2):(2-4):(2-4).

8. The method for preparing a two-component polyurethane coating for decorative panels according to claim 1, characterized in that: The preparation method of the fluorinated diol comprises the following steps: adding isophorone diisocyanate into a reaction container, preheating to 65° C. under a nitrogen atmosphere, adding tetrafluoropropanol and dibutyltin dilaurate, heating to 90-91° C. for reaction for 2-3 hours, adding trihydroxypropane, and keeping the temperature to react until the isocyanate group content in the system reaches a theoretical value, thereby obtaining the fluorinated diol; In the fluorinated diol, the molar ratio of isophorone diisocyanate:tetrafluoropropanol:trihydroxypropane is 1:1:

1.

9. The method for preparing a two-component polyurethane coating for decorative panels according to claim 1, characterized in that: The preparation method of trisilanol POSS comprises the following steps: adding lithium hydroxide and deionized water into tetrahydrofuran, stirring at room temperature for 10-15 minutes, adding phenyltriethoxysilane, controlling the dropping time, heating to 38-40° C. for reaction for 24-36 hours, and post-processing to obtain trisilanol POSS.

10. A two-component polyurethane coating prepared according to the method for preparing a two-component polyurethane coating for a decorative plate material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Hyperbranched aqueous polyurethane and preparation thereof

    CN101440150A

  • Waterborne fluorine-containing polyurethane resin capable of being cured by UV (Ultraviolet) and preparation method of waterborne fluorine-containing polyurethane resin

    CN104231228A

  • Ultraviolet photocuring coating containing inorganic pigment and filler and preparation method thereof

    CN104693994A

  • Super-hydrophobic polyurethane coating and preparation method thereof

    CN107286318A

  • Preparation method of environment-UV gloss oil for food packaging and printing

    CN107652874A

Cited By

  • High-strength light-weight packaging carton and preparation method thereof

    CN120590823A

  • A high-strength lightweight packaging carton and a method for manufacturing the same

    CN120590823B