Graphene modified edge sealing adhesive with high barrier property and preparation method thereof
By introducing graphene modified materials into the edge sealing glue of electronic paper, a high barrier performance edge sealing glue is formed, which solves the problem of electronic paper performance failure caused by water vapor transmission in the prior art, and achieves a longer period of stable operation. and moisture and heat resistance.
Patent Information
- Application Number
- CN202411306436.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-15
AI Technical Summary
During long-term use, the existing epoxy edge sealing glue fails due to the passing of water vapor, and edge damage occurs in only 1,000 hours of aging test, which cannot meet the needs of efficient operation for longer periods of time.
Using graphene modified edge sealing glue with high barrier properties, the water vapor of the glue is enhanced by synthesizing bisphenol F-type epoxy resin and modified epoxy resin, ethylenediamine bissalicylic acid amide glycidyl ether, graphene and other materials. Barrier properties, forming a sheet-like structure to reduce transmittance.
It significantly reduces the water vapor transmission rate, keeps the edge sealing glue stable during the 2000-hour aging test, provides excellent moisture and heat resistance and adhesive properties, and extends the service life of electronic paper.
Smart Images

Figure BDA0005049359290000011 
Figure BDA0005049359290000021 
Figure BDA0005049359290000051
Abstract
Description
Technical Field
[0001] The present invention relates to the field of display screens, and is mainly applied to electronic paper display screens, and in particular to a graphene-modified edge-sealing adhesive with high barrier properties and a preparation method thereof. Background Art
[0002] Electronic ink is a material that is easily affected by water vapor and oxygen, which can lead to performance failure. It needs to be protected by packaging materials with high barrier properties to ensure its stable operation. At present, the main liquid packaging material is epoxy edge sealant. However, barrier performance has become the main factor limiting the long-term and efficient operation of electronic paper. There are tiny pores inside the glue. As time goes by, water vapor will pass through the glue layer along the pores, causing the electronic ink to fail. The aging test of epoxy edge sealants on the market is mainly 1000 hours, and the electronic paper screen will have edge damage. Summary of the invention
[0003] The invention provides a graphene-modified edge sealing adhesive with high barrier performance. By synthesizing an epoxy resin with high barrier performance and adding graphene with a flaky structure, the water vapor barrier performance of the adhesive is enhanced. Compared with the common epoxy edge sealing adhesives on the market, the water vapor permeability is greatly reduced, and the sample after edge sealing can pass the aging test for 2000 hours.
[0004] In order to achieve the purpose, the present invention adopts the following technical scheme:
[0005] A graphene-modified edge sealing adhesive with high barrier performance is characterized in that the raw materials are composed of 60-80 parts of bisphenol F epoxy resin, 10-30 parts of modified epoxy resin, 5-10 parts of epoxy diluent, 1-2 parts of silane coupling agent, 0.1-0.3 parts of defoaming agent, 10-20 parts of graphene, 1-3 parts of titanium dioxide, 0.5-1.5 parts of thixotropic agent and 25-35 parts of mixed amine in parts by weight.
[0006] Furthermore, the modified epoxy resin is ethylenediamine disalicylic acid amide glycidyl ether, which is prepared by the following steps:
[0007] 1) Phenyl salicylate and ethylenediamine are added into a reactor in a mass ratio of (7-7.2):1, heated and stirred to 150-160° C. under nitrogen protection, and the mixture is kept warm and stirred until the reaction of phenyl salicylate is complete as detected by HPLC, and the byproduct phenol is removed in vacuo, and the product is then added into ethanol for recrystallization to obtain the product ethylenediamine disalicylic acid amide.
[0008] The reaction formula of the above reaction is:
[0009]
[0010] 2) epichlorohydrin and the product ethylenediamine disalicylic acid amide in step 1) are added to a reactor in a mass ratio of (3-3.2):1 and heated to 55-65° C. with stirring, and a sodium hydroxide aqueous solution (mass concentration of 15-30%) accounting for 50%-55% of the total mass of the raw materials is uniformly added dropwise within 0.8-1.2 hours. After the addition is completed, the reaction is continued at a constant temperature of 55-65° C. for 1.5-2.5 hours, and then dichloromethane accounting for 55%-65% of the total mass of the raw materials is added. After standing and stratification, the water layer is removed, and then it is repeatedly washed with water for 3 times, and vacuum concentrated to obtain the product ethylenediamine disalicylic acid amide glycidyl ether.
[0011] The reaction formula of the above reaction is:
[0012]
[0013] Furthermore, the epoxy diluent is at least one of 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether and polypropylene glycol diglycidyl ether.
[0014] Furthermore, the mixed amine is a mixture of polyetheramine and 1-methyl-2,4-cyclohexanediamine. Preferably, the mass ratio of polyetheramine to 1-methyl-2,4-cyclohexanediamine is (2-2.5):1.
[0015] Furthermore, the silane coupling agent is γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane or N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.
[0016] Furthermore, the defoaming agent is a silicone polymer, such as BYK-066N, Deqian 6800, and QM2068.
[0017] Furthermore, the titanium dioxide is anatase titanium dioxide or rutile titanium dioxide.
[0018] Furthermore, the thixotropic agent is fumed silica, such as Cabot TS-610 and Wacker H-30RM.
[0019] The method for preparing the graphene-modified edge sealing adhesive with high barrier performance of the present invention comprises the following steps:
[0020] Step 1, after mixing bisphenol F epoxy resin, modified epoxy resin, epoxy diluent, silane coupling agent, defoaming agent, titanium dioxide, graphene and thixotropic agent according to a proportion, high-speed dispersion is carried out at a speed of 2000-3000 r / min for 30-40 minutes, and vacuum degassing is carried out to obtain material A;
[0021] Step 2: After material A is cooled to room temperature, add mixed amine, disperse at a low speed of 800-1200 r / min for 20-25 minutes, vacuum degas, filter and package to obtain graphene modified edge sealing adhesive with high barrier performance, and store at -40°C.
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0023] 1. The epoxy resin used in the edge sealing glue of the present invention is a mixture of bisphenol F epoxy resin and bis(ethylenediamine disalicylic acid amide glycidyl ether), wherein: by synthesizing bis(ethylenediamine disalicylic acid amide glycidyl ether, the system obtains excellent moisture and heat resistance, so that the glue can have excellent barrier ability to water vapor under long-term high temperature and high humidity environment, and at the same time, bis(ethylenediamine disalicylic acid amide glycidyl ether has relatively high activity, which can reduce the curing temperature of the system; low-viscosity bisphenol F resin can ensure that the glue has a lower viscosity at room temperature, which is conducive to vacuum degassing, and also makes the system have good fluidity.
[0024] 2. The mixed amine used in the edge sealing glue of the present invention is a mixture of polyetheramine and 1-methyl-2,4-cyclohexanediamine, wherein: the cyclic structure of 1-methyl-2,4-cyclohexanediamine can ensure the barrier performance of the system and effectively reduce the water vapor permeability of the glue; through the compounding of polyetheramine and 1-methyl-2,4-cyclohexanediamine, the operation time and curing time of the glue are balanced.
[0025] 3. The graphene added to the edge sealing glue of the present invention has a flaky structure, and the barrier properties of the glue can be further reduced by stacking the flaky structures.
[0026] 4. The edge sealing adhesive of the present invention has excellent bonding performance and good thermal stability, and is green, environmentally friendly and harmless to the human body. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The viscosity changes of the packaging glue of each embodiment and comparative example of the present invention within 4 hours after thawing at room temperature (25° C.) for 1 hour (the viscosity of the glue was tested every half an hour).
[0028] Figure 2 The curing time of the edge sealing adhesive of each embodiment of the present invention at 65° C. and 70° C. DETAILED DESCRIPTION
[0029] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings. The following content is only an example and explanation of the concept of the present invention. The technicians in the relevant technical field make various modifications or supplements to the specific implementation cases described or replace them with similar methods. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0030] The graphene used in the following examples can be prepared according to the method disclosed in patent CN 104609413 B, or can be purchased directly from Hefei Microcrystalline Material Technology Co., Ltd.
[0031] Example 1
[0032] In this embodiment, ethylenediamine disalicylic acid amide glycidyl ether is first prepared according to the following steps:
[0033] 1) 214 parts by weight of phenyl salicylate (CAS No.: 118-55-8) and 30 parts by weight of ethylenediamine (CAS No.: 107-15-3) were added to a reactor, heated and stirred to 155° C. under nitrogen protection, and continued to be heated and stirred until phenyl salicylate was completely reacted as detected by HPLC, and the by-product phenol was removed in vacuo, and the product was then added to ethanol for recrystallization to obtain the product ethylenediamine disalicylic acid amide.
[0034] 2) 370 parts by weight of epichlorohydrin (CAS No.: 106-89-8) and 120 parts by weight of the product ethylenediamine disalicylic acid amide in step 1) are added to a reactor and heated to 60° C. with stirring; 250 parts by weight of an aqueous sodium hydroxide solution (mass concentration of 20%) is uniformly added dropwise within 1 hour with constant temperature stirring; after the addition is completed, the mixture is kept at a constant temperature of 60° C. for 2 hours, and then 300 parts by weight of dichloromethane (CAS No.: 75-09-2) is added, and the water layer is removed after standing for stratification, and then the mixture is repeatedly washed with water for 3 times, and vacuum concentrated to obtain the product ethylenediamine disalicylic acid amide glycidyl ether.
[0035] In this embodiment, the edge sealing adhesive is prepared according to the following steps:
[0036] 1) 70 parts of bisphenol F epoxy resin (Anhui Xinyuan XY170L), 20 parts of bis(ethylenediamine) disalicylic acid amide glycidyl ether, 8 parts of epoxy diluent 1,4-butanediol diglycidyl ether (Anhui Xinyuan 622), 2 parts of silane coupling agent (γ-aminopropyltriethoxysilane), 0.2 parts of defoaming agent (QM-2068), 1 part of thixotropic agent (Wake H30RM), 2 parts of titanium dioxide (DuPont R902) and 20 parts of graphene were dispersed at a speed of 3000 r / min for 30 minutes, and vacuum degassed to obtain material A.
[0037] 2) After material A is cooled to room temperature, 20 parts by mass of polyetheramine (Huntsman D230) and 10 parts by mass of 1-methyl-2,4-cyclohexanediamine (Xiamen Geruida) are added, and the mixture is dispersed at a low speed of 1000 r / min for 20 minutes, vacuum degassed, filtered and packaged to obtain a graphene-modified edge sealing adhesive with high barrier properties, which is stored at -40°C.
[0038] Example 2
[0039] In this embodiment, the edge sealing adhesive is prepared in the same manner as in Example 1, except that the mass fraction of bisphenol F epoxy resin is changed to 80 parts, and the mass fraction of bis(ethylenediamine) disalicylic acid amide glycidyl ether is changed to 10 parts.
[0040] Example 3
[0041] In this embodiment, the edge sealing adhesive is prepared in the same manner as in Example 1, except that the mass fraction of bisphenol F epoxy resin is changed to 60 parts, and the mass fraction of bis(ethylenediamine) disalicylic acid amide glycidyl ether is changed to 30 parts.
[0042] Comparative Example 1
[0043] In this comparative example, the edge sealing adhesive was prepared in the same manner as in Example 1, except that the mass fraction of bisphenol F epoxy resin was changed to 45 parts, and the mass fraction of bis(ethylenediamine) disalicylic acid amide glycidyl ether was changed to 45 parts.
[0044] Comparative Example 2
[0045] In this comparative example, the edge sealing adhesive was prepared in the same manner as in Example 1, except that no diethylenediamine disalicylic acid amide glycidyl ether was added to the system, and the mass fraction of bisphenol F epoxy resin was 90 parts.
[0046] Comparative Example 3
[0047] In this comparative example, an edge sealing adhesive was prepared in the same manner as in Example 1, except that 20 parts by mass of polyetheramine and 10 parts by mass of 1,3-cyclohexanedimethylamine were added in step 2) instead of adding 1-methyl-2,4-cyclohexanediamine.
[0048] Comparative Example 4
[0049] In this comparative example, the edge sealing adhesive was prepared in the same manner as in Example 1, except that graphene and bis(ethylenediamine) disalicylic acid amide glycidyl ether were not added to the system, and the mass fraction of bisphenol F epoxy resin was 90 parts.
[0050] The following performance tests were performed on the edge sealing adhesives of each embodiment and comparative example:
[0051] 1. Water permeability test
[0052] The epoxy edge sealing adhesive of each embodiment and comparative example was made into a film with a thickness of 0.25 mm using a four-sided preparation device. After the glue was completely cured (>7 days), the prepared film was packaged at the mouth of a bottle filled with water, and placed in a constant temperature and humidity circulation box (temperature 60°C, humidity 100%) for 24 hours. The water permeability of the glue was tested (test standard: ASTME-96). The results are shown in Table 1.
[0053] Table 1 24-hour water permeability of edge sealing adhesive prepared in each embodiment (temperature 50°C, humidity 100%)
[0054]
[0055] It can be seen from Table 1 that due to the introduction of bis(ethylenediamine) disalicylic acid amide glycidyl ether into the system, the moisture and heat resistance of the edge sealing glue is enhanced, and at the same time, the ring structure of 1-methyl-2,4-cyclohexanediamine introduced in the curing agent can further enhance the barrier performance of the system. The graphene in the glue has a sheet structure, and after stacking each other, the water permeability of the system is further reduced. Therefore, the water permeabilities of Examples 1, 2, 3 and Comparative Example 1 are all around 2.5, while the water permeability of Comparative Example 2 without adding bis(ethylenediamine) disalicylic acid amide glycidyl ether is increased to 10, the water permeability of Comparative Example 3 in which 1-methyl-2,4-cyclohexanediamine is replaced by 1,3-cyclohexanedimethylamine reaches 8, and the water permeability of Comparative Example 4 without adding graphene and bis(ethylenediamine) disalicylic acid amide glycidyl ether is increased to more than 20.
[0056] 2. Damp heat aging test
[0057] After the glue is completely cured (>7 days), the packaged test piece is placed in a constant temperature and humidity cycle box to test its sealing performance (temperature 60°C, humidity: 80%). The result is mainly reflected by whether the internal packaged test paper turns red (if the packaging effect is not good, water vapor will enter it and the internal packaged test paper will turn red). The condition of the packaged test piece is observed every 250 hours.
[0058] The packaging simulation test results show that the edge sealing adhesive provided in Examples 1 to 3 of the present invention does not cause the test paper packaged inside to change color after 1500 hours at a temperature of 60° C. and a humidity of 80%.
[0059] 3. Viscosity change test
[0060] The packaging glue prepared in each embodiment and comparative example was taken out from a -40°C freezer, thawed at room temperature for 1 hour, and then the viscosity change of the glue within 4 hours was tested (the viscosity of the glue was tested every half an hour). The results are as follows: Figure 1 shown.
[0061] from Figure 1It can be seen that the edge sealing glue with too high proportion of diethylenediamine disalicylic acid amide glycidyl ether (Comparative Example 1) changes viscosity rapidly at room temperature. By adjusting the ratio of diethylenediamine disalicylic acid amide glycidyl ether to bisphenol F type epoxy resin, the curing time and viscosity change of the edge sealing glue can be effectively balanced.
[0062] 4. Curing time test
[0063] The test paper that changes color easily due to moisture is encapsulated with the epoxy glue prepared in each embodiment and comparative example by using a glue dispenser. The encapsulated test piece is placed in an oven at 65°C and 70°C to test the curing time of the glue. The test results are shown in FIG. Figure 2 .
[0064] from Figure 2 It can be seen that the edge sealing glue provided by the present invention, by adding diethylenediamine disalicylic acid amide glycidyl ether to the formula system, can achieve rapid curing of the glue in 1 hour under heating (65°C); compared with the system without adding diethylenediamine disalicylic acid amide glycidyl ether (Comparative Example 4), the curing speed is significantly faster, and the viscosity of the glue changes slowly at room temperature ( Figure 1 ), while when the ratio of bis(ethylenediamine) disalicylic acid amide glycidyl ether is high (Comparative Example 1), the curing speed is faster, but the viscosity changes significantly faster ( Figure 1 ), by adjusting the ratio of diethylenediamine disalicylic acid amide glycidyl ether to bisphenol F type epoxy resin, the curing time and viscosity change of the edge sealing adhesive are balanced.
[0065] In summary, the present invention provides a graphene-modified edge-sealing adhesive with high barrier performance: by introducing bisphenol F epoxy resin to enhance the flowability of the system; by synthesizing bis(ethylenediamine) disalicylic acid amide glycidyl ether to enhance the moisture and heat resistance of the system and accelerate the curing speed of the system; by introducing 1-methyl-2,4-cyclohexanediamine with a ring structure to further enhance the barrier ability of the system to water vapor, and at the same time, by adding graphene and stacking its sheet structure, the glue has better water-insulating performance. The edge-sealing adhesive has excellent water vapor barrier effect while being cured at 65°C, effectively reducing the damage caused by water vapor erosion to components.
[0066] The above description is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make corresponding adjustments and improvements without departing from the principles of the present invention. These adjustments and improvements should also be regarded as the scope of protection of the present invention.
Claims
1. A graphene-modified edge sealing adhesive with high barrier properties, characterized in that: The composition of the raw materials in parts by weight is: 60-80 parts of bisphenol F epoxy resin, 10-30 parts of modified epoxy resin, 5-10 parts of epoxy diluent, 1-2 parts of silane coupling agent, 0.1-0.3 parts of defoaming agent, 10-20 parts of graphene, 1-3 parts of titanium dioxide, 0.5-1.5 parts of thixotropic agent and 25-35 parts of mixed amine.
2. The graphene-modified edge sealing adhesive with high barrier properties according to claim 1, characterized in that: The modified epoxy resin is ethylenediamine disalicylic acid amide glycidyl ether.
3. The graphene-modified edge sealing adhesive with high barrier properties as claimed in claim 2, characterized in that: The ethylenediamine disalicylic acid amide glycidyl ether is prepared by the following steps: 1) adding phenyl salicylate and ethylenediamine in a mass ratio of 7 to 7.2:1 into a reactor, heating and stirring to 150 to 160° C. under nitrogen protection, continuing to keep warm and stir until phenyl salicylate reacts completely, removing the byproduct phenol in vacuo, and then adding the product to ethanol for recrystallization to obtain the product ethylenediamine disalicylic acid amide; 2) epichlorohydrin and the product ethylenediamine disalicylic acid amide in step 1) are added to a reactor in a mass ratio of 3 to 3.2:1 and heated to 55 to 65° C. with stirring, and a sodium hydroxide aqueous solution with a mass concentration of 15 to 30% accounting for 50% to 55% of the total mass of the raw materials is uniformly added dropwise within 0.8 to 1.2 hours. After the addition is completed, the reaction is continued at a constant temperature for 1.5 to 2.5 hours, and then dichloromethane accounting for 55% to 65% of the total mass of the raw materials is added. After standing and stratification, the water layer is removed, and then it is repeatedly washed with water, and vacuum concentrated to obtain the product ethylenediamine disalicylic acid amide glycidyl ether.
4. The graphene-modified edge sealing adhesive with high barrier properties according to claim 1, characterized in that: The epoxy diluent is at least one of 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether and polypropylene glycol diglycidyl ether.
5. The graphene-modified edge sealing adhesive with high barrier properties according to claim 1, characterized in that: The silane coupling agent is γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane or N-(2-aminoethyl)-3-aminopropyltrimethoxysilane; the defoaming agent is an organic silicon polymer; the titanium dioxide is anatase titanium dioxide or rutile titanium dioxide; and the thixotropic agent is fumed silica.
6. The graphene-modified edge sealing adhesive with high barrier properties according to claim 1, characterized in that: The mixed amine is a mixture of polyetheramine and 1-methyl-2,4-cyclohexanediamine.
7. The graphene-modified edge sealing adhesive with high barrier properties as claimed in claim 6, characterized in that: The mass ratio of polyetheramine to 1-methyl-2,4-cyclohexanediamine is 2-2.5:
1.
8. A method for preparing the graphene-modified edge sealing adhesive with high barrier properties as claimed in any one of claims 1 to 7, characterized in that: The steps include: Step 1, after mixing bisphenol F epoxy resin, modified epoxy resin, epoxy diluent, silane coupling agent, defoaming agent, titanium dioxide, graphene and thixotropic agent according to a proportion, high-speed dispersion is carried out at a speed of 2000-3000 r / min for 30-40 minutes, and vacuum degassing is carried out to obtain material A; Step 2: After material A is cooled to room temperature, add mixed amine, disperse at a low speed of 800-1200 r / min for 20-25 minutes, vacuum degas, filter and package to obtain graphene modified edge sealing adhesive with high barrier performance, and store at -40°C.