Method for vanadium extraction and dephosphorization of molten iron and low-phosphorus semi-steel

Through the combination of induction furnace and vanadium extraction and dephosphorization treatment agent, the problem of difficulty in removing phosphorus by vanadium extraction and semi-steel is solved, the quality of semi-steel is improved, green production and environmental protection are achieved, and production costs are reduced.

CN118957308APending Publication Date: 2024-11-15PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411170955.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The waste gas pollution in the existing vanadium extraction and dephosphorization process is severe, and the wastewater treatment is difficult, and different ores require different vanadium extraction technologies and process conditions, which increases the technical complexity and difficulty, and does not involve induction furnaces and vanadium extraction and dephosphorization treatment agents. Combined with the solution.

Method used

The induction furnace is combined with vanadium-elevating dephosphorization treatment agent (including manganese ore, magnesium sand and iron red), and the electromagnetic stirring force is provided through the insulation current of the induction furnace, and the slag gold reaction is carried out to effectively remove the phosphorus element in half steel. , obtain low phosphorus half steel.

Benefits of technology

The quality of semi-steel is significantly improved, the impact of phosphorus elements on the environment is reduced, green production is achieved, the dephosphorization pressure of subsequent converter steelmaking is reduced, and product adaptability and market competitiveness are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957308A_ABST
    Figure CN118957308A_ABST
Patent Text Reader

Abstract

The method comprises the steps that after the molten iron is heated through an induction furnace, a vanadium extraction and dephosphorization treatment agent is added, power supply parameters of the induction furnace are adjusted to be in a heat preservation level, electromagnetic stirring force is provided through current of the heat preservation level to conduct slag-metal reaction, vanadium slag is removed after the reaction is finished, and the low-phosphorus semi-steel is obtained. And the low-phosphorus semisteel is conveyed to a steelmaking converter for steelmaking. According to the method, the problem of difficulty in phosphorus removal of vanadium extraction semisteel of a steel plant is solved by combining the induction furnace and the vanadium extraction and dephosphorization treatment agent, so that the quality of the semisteel is remarkably improved, the semisteel better meets the use requirements, the product adaptability is improved, the phosphorus element in the slag is timely removed, the influence of the phosphorus element on the environment can be reduced, and the service life of the semisteel is prolonged. And green production is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a method for extracting vanadium and dephosphorizing molten iron and a low-phosphorus semi-steel. Background Art

[0002] my country is a major producer of vanadium-titanium magnetite. Many large enterprises use vanadium-titanium magnetite for smelting. The molten iron smelted in blast furnaces has a higher vanadium content than ordinary molten iron. Vanadium is an important resource, so vanadium must be extracted from molten iron before steelmaking to produce vanadium slag. At present, there are many production methods for producing vanadium slag at home and abroad, mainly including New Zealand's ladle vanadium blowing process, South Africa's shaking ladle vanadium extraction process, Russia and China's converter vanadium extraction process, etc. Other vanadium extraction processes include vanadium extraction from vanadium-containing steel slag and stone coal vanadium extraction process.

[0003] The silicon and manganese content of the semi-steel obtained after vanadium extraction is only trace, which results in slag formation and less heat-generating elements during converter steelmaking, making slag formation difficult and dephosphorization extremely difficult. However, it is precisely because of this feature of semi-steel that it also provides good conditions for dephosphorization before the converter: there is no need to carry out desiliconization treatment before dephosphorization.

[0004] In order to control the phosphorus content of molten steel, various treatment methods have been developed since 1980: ① Pre-dephosphorization in molten iron ladle or torpedo car; ② Pre-dephosphorization of molten iron in special converter; ③ Deep dephosphorization in converter steelmaking process; ④ Reducing phosphorus reversion in ladle refining process. At present, these methods have been successfully applied in industry. Since 1990, most steel enterprises in Japan and South Korea have adopted the process of pre-dephosphorization of molten iron in special converter, while my country has basically adopted the process of dephosphorization in converter steelmaking, and few have adopted pre-dephosphorization of molten iron. Baosteel only pre-dephosphorizes in torpedo tanks when producing low-phosphorus steel. At present, many steel enterprises use the injection method for desulfurization, so desulfurization and dephosphorization can be carried out at the same station to reduce the task of subsequent converter steelmaking dephosphorization.

[0005] For example, the Chinese patent application number CN201310087587.X discloses "a treatment agent for desulfurization and dephosphorization of molten steel and a preparation method thereof", and the chemical composition weight percentage of the treatment agent is: iron oxide FeO+Fe 2 O 3 :15-25%; Lithium metal or compound 10-20%; CaF 2 :5%-10%; Al2O 3 : 8%-15%; mixed rare earth: 0.5-2%, the rest is CaO. The metal lithium or compound is Li, Li 2 O, LiOH, Li 2 CO 3The preparation method comprises the following steps: ball-milling the raw materials and pre-firing the mixture, wherein the pre-firing temperature is 1100° C. to 1200° C.; crushing the pre-firing raw material mixture into a particle size range of 1 to 2 mm, and then stirring and mixing the mixture evenly.

[0006] For example, Chinese patent application number CN201310502990.4 discloses "a method for simultaneously desulfurizing and dephosphorizing semi-steel", wherein the semi-steel is sprayed with a desulfurization oxygen lance in the first stage, and the spray material is a blowing powder with an inert gas as a carrier; the semi-steel is sprayed with a desulfurization lance in the second stage, and the spray material is a mixture of blowing powder with an inert gas as a carrier and passivation magnesium powder; the semi-steel is sprayed with a desulfurization oxygen lance in the third stage, and the spray material is a blowing powder with an inert gas as a carrier, wherein the semi-steel is molten iron obtained after vanadium-containing molten iron is extracted from vanadium in a converter, and the blowing powder is made of 55 to 80 parts by weight of passivating lime, 5 to 15 parts of iron oxide and 20 to 30 parts of sodium oxide.

[0007] For example, the Chinese patent application number CN200510071571.5 discloses "large-scale desulfurization of molten iron in front of the furnace or three desulfurizations at the same time to completely liberate the blast furnace and converter", a new molten iron pretreatment process that spreads soda on the molten iron gushing out of the sand outlet of the iron-making yard to significantly desulfurize, dephosphorize and desiliconize, and even to extract vanadium when smelting vanadium-titanium ore.

[0008] For example, the Chinese patent application number CN200610161323.4 discloses a "refining agent for desulfurization and dephosphorization of molten steel outside the furnace", which contains BaO 35-70, BaF 2 10~35, MnO 5~13, CaO4~10, Al 2 O 3 The remainder of 2 to 10 is impurities and binders.

[0009] For example, the Chinese patent application number CN200810048090.6 discloses a "composite slag for simultaneous desulfurization and dephosphorization of stainless steel by return process". The composite slag includes the following components and weight ratios: when the CaO content is 1 part, BaO and / or BaCO 3 0.6~1.8 parts, CaF 2 and / or BaCl 2 0.3~0.6 parts, Fe 2 O 3 0.10~0.15 parts. When lime is used as CaO raw material, the CaO content in the lime is greater than 92%, the sulfur content is less than 0.025%, and the silicon dioxide content is less than 1%. The purity of other components is required to be above 98%. The particle size of the composite slag is less than 1cm 3 .

[0010] The vanadium extraction and dephosphorization methods mentioned in the above schemes have serious waste gas pollution and difficult to treat wastewater pollution. Both pyrometallurgical and hydrometallurgical vanadium extraction technologies have certain selectivity for ores. Different ores may require different vanadium extraction technologies and process conditions, which increases the complexity and difficulty of technical application. The above schemes do not involve the technical solution of combining induction furnaces with vanadium extraction and dephosphorization treatment agents for vanadium extraction and dephosphorization. In view of this, improvements should be made to the existing technology. Summary of the invention

[0011] The main purpose of the present invention is to provide a method for vanadium extraction and dephosphorization of molten iron and low-phosphorus semi-steel, which solves the problem of difficulty in removing phosphorus from vanadium extraction semi-steel in steel plants by combining an induction furnace with a vanadium extraction and dephosphorization treatment agent, thereby significantly improving the quality of the semi-steel, making it more in line with use requirements, increasing the adaptability of the product, and timely removing the phosphorus element in the slag can also reduce the impact of the phosphorus element on the environment, thereby realizing green production.

[0012] According to one aspect of the present invention, a method for vanadium extraction and dephosphorization of molten iron is provided, which comprises heating the molten iron with an induction furnace, adding a vanadium extraction and dephosphorization treatment agent, adjusting the power supply parameter of the induction furnace to the insulation gear, using the insulation gear current to provide electromagnetic stirring force for slag-metal reaction, and removing the vanadium slag after the reaction is completed to obtain low-phosphorus semi-steel and transport it to a steelmaking converter for steelmaking. According to one embodiment of the present invention, high-carbon scrap steel is scrap steel with a carbon content of >0.75%.

[0013] According to one embodiment of the present invention, the vanadium extraction and dephosphorization treatment agent includes manganese ore, magnesia and red iron.

[0014] According to one embodiment of the present invention, in terms of weight percentage, Mn in manganese ore is greater than 30%, MgO in magnesia is greater than 80%, and TFe in red iron is greater than 60%.

[0015] According to one embodiment of the present invention, the particle size range of manganese ore, magnesia and red iron ore is 1-5 mm.

[0016] According to one embodiment of the present invention, manganese ore, magnesia and red iron ore are fully mixed in a weight ratio of 1-2:1-1.5:6.5-8.

[0017] According to one embodiment of the present invention, adjusting the power supply parameters of the induction furnace to the insulation gear includes determining whether the induction furnace is in the insulation gear by detecting the working state of the induction furnace, where the working state includes real-time temperature and / or heating speed.

[0018] According to one embodiment of the present invention, the heating includes heating to 1360-1400°C.

[0019] According to one embodiment of the present invention, the amount of vanadium extraction and dephosphorization agent added is 30-50 kg / (t iron).

[0020] According to one embodiment of the present invention, the reaction time of the slag-gold reaction is 20 to 30 minutes.

[0021] According to another aspect of the present invention, a low-phosphorus semi-steel is provided, which is prepared by using any one of the methods in the above technical solutions.

[0022] In a method for extracting vanadium and dephosphorizing molten iron according to an embodiment of the present invention, an induction furnace and a vanadium extraction and dephosphorization treatment agent are combined to solve the problem of difficulty in removing phosphorus from vanadium-extracted semi-steel in steel plants, thereby significantly improving the quality of the semi-steel and making it more in line with use requirements, increasing the adaptability of the product, and timely removing the phosphorus element in the slag can also reduce the impact of the phosphorus element on the environment, thereby achieving green production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 A process flow chart of a method for extracting vanadium and dephosphorizing molten iron according to an exemplary embodiment of the present invention is shown. DETAILED DESCRIPTION

[0025] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

[0026] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.

[0027] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0028] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0029] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0030] Technologies, methods, and apparatus known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and apparatus should be considered part of the specification.

[0031] like Figure 1 As shown, the present invention provides a method for extracting vanadium and dephosphorizing molten iron, which includes heating the molten iron with an induction furnace and then adding a vanadium extraction and dephosphorization treatment agent, adjusting the power supply parameters of the induction furnace to a heat preservation gear, using the heat preservation gear current to provide an electromagnetic stirring force to perform a slag-metal reaction, and after the reaction is completed, removing the vanadium slag to obtain a low-phosphorus semi-steel and transporting it to a steelmaking converter for steelmaking.

[0032] In the method for vanadium extraction and dephosphorization of molten iron according to the embodiment of the present invention, the induction furnace and the vanadium extraction and dephosphorization treatment agent are combined to solve the problem of difficulty in removing phosphorus from vanadium-extracted semi-steel in steel plants, thereby significantly improving the quality of semi-steel, making it more in line with the use requirements, increasing the adaptability of the product, and timely removing the phosphorus element in the slag can also reduce the impact of phosphorus on the environment, thereby achieving green production. The present invention is suitable for enterprises that use vanadium-containing molten iron for vanadium extraction, and can effectively remove the phosphorus content of semi-steel while extracting vanadium, which is conducive to reducing the dephosphorization pressure of semi-steel converter steelmaking, creating good conditions for converter low-slag steelmaking, and helping to reduce the production cost of steelmaking.

[0033] In some specific embodiments, the vanadium extraction and dephosphorization treatment agent includes manganese ore, magnesia and iron oxide. In the process of vanadium extraction from molten iron, manganese ore, magnesia and iron oxide are used as vanadium extraction and dephosphorization treatment agents, and their ratios are preset. Under suitable conditions, the oxidation and extraction of vanadium can be effectively promoted, and the extraction rate of vanadium in molten iron can be significantly improved. The components in manganese ore, magnesia and iron oxide react chemically with phosphorus in molten iron at high temperature to generate stable phosphate compounds, thereby achieving dephosphorization. The main function of iron oxide is to oxidize vanadium and phosphorus in molten iron, while manganese ore and magnesia mainly provide MnO and MgO, so that the oxidized V 2 O 3 , P 2 O 5 It can form slag with it, thereby achieving effective removal of vanadium and phosphorus.

[0034] In some specific embodiments, by weight percentage, Mn>30% in manganese ore, MgO>80% in magnesia, and TFe>60% in iron oxide red. Comprehensively considering multiple aspects such as formula design, raw material selection, production process control, and finished product analysis and testing, through scientific methods and rigorous experimental verification, the performance of the treatment agent meets actual needs and achieves the best effect, thereby obtaining the content of each main component, Mn>30% in manganese ore, MgO>80% in magnesia, and TFe>60% in iron oxide red.

[0035] On the basis of the above embodiments, the particle size range of manganese ore, magnesia and iron red is 1 ~ 5mm. In order to improve the efficiency of vanadium extraction and dephosphorization process, the particle size of each substance in the vanadium extraction and dephosphorization treatment agent should be reduced. Reducing the particle size means that the treatment agent per unit mass or volume has a larger surface area, thereby increasing the contact area between the treatment agent and molten iron or slag. Larger contact area is conducive to the progress of vanadium extraction and dephosphorization reaction, and improves reaction rate and efficiency. After the particle size is reduced, the diffusion path between the reactants is also shortened accordingly, so that the reactants can reach the reaction interface faster and participate in the reaction, further improving the reaction efficiency. The reactants with small particle size can also improve the reaction kinetics conditions, making the reaction easier to carry out at lower temperature and pressure, thereby saving energy and reducing production costs.

[0036] In order to further improve the vanadium extraction rate and dephosphorization rate, based on the above examples, manganese ore, magnesia and iron oxide are fully mixed in a weight ratio of 1-2:1-1.5:6.5-8. Increasing the amount of reactants in the reaction system can increase the collision frequency between molecules, thereby improving the vanadium extraction rate, dephosphorization rate and reducing the impact of the treatment agent on other components in the molten iron. The FeO provided by iron oxide not only oxidizes vanadium and phosphorus, but also needs to react with V 2 O 3 A vanadium spinel phase is formed, and MnO and MgO participate in forming a phosphorus-containing phase, and their weight ratio is designed in proportion to the requirements of the formed phase.

[0037] The temperature range set in the insulation gear is usually relatively low, aiming to maintain the temperature of the reaction system in the furnace in a relatively stable and low range to prevent overheating or too fast cooling. On the basis of the above embodiments, adjusting the power supply parameters of the induction furnace to the insulation gear includes determining whether the induction furnace is in the insulation gear by detecting the working state of the induction furnace, and the working state includes one or more of the real-time temperature and the heating speed. In the insulation gear, the power output of the induction furnace will be relatively low to reduce energy consumption and avoid overheating. When the real-time temperature and the heating speed reach the preset state, and the temperature in the furnace no longer rises when the heating continues, it is the insulation gear.

[0038] Based on the above embodiments, the temperature range after heating is 1360~1400℃. Adding the vanadium extraction and dephosphorization agent after reaching this temperature range helps to ensure uniform temperature distribution in the reaction system and avoid local overheating or supercooling, which is crucial to maintaining the stability of the reaction rate and improving the purity of the product.

[0039] The amount of vanadium extraction and dephosphorization treatment agent added must be sufficient and accurate to ensure that the expected process effect is achieved. This treatment agent plays a vital role in metallurgical or chemical processes. It can effectively react with the vanadium and phosphorus elements in the raw materials, thereby separating them from the main material. In order to achieve this goal, the control of the amount added is crucial. If the amount added is insufficient, the treatment agent may not be able to fully react with all vanadium and phosphorus elements, resulting in some impurities remaining, affecting the quality and performance of the final product. On the contrary, if the amount added is too much, although the complete removal of vanadium and phosphorus can be ensured, it will also bring unnecessary waste and increase production costs. At the same time, excessive treatment agents may also have an adverse effect on the reaction system, such as changing reaction conditions, introducing new impurities or increasing the complexity of subsequent treatment. On the basis of the above embodiment, the amount of vanadium extraction and dephosphorization treatment agent added is 30~50kg / (t iron).

[0040] In actual production, it is necessary to accurately calculate and set the necessary reaction time according to the specific conditions of the reaction (such as temperature, pressure, stirring intensity, reactant concentration, etc.) and the requirements of the target product. The reaction time must be long enough to ensure that all key reaction steps can be completed thoroughly to achieve the expected reaction effect. At the same time, in order to optimize production efficiency, it is also necessary to shorten unnecessary reaction time as much as possible while ensuring the reaction effect, so as to reduce energy consumption and production costs. Based on the above embodiment, the reaction time of the slag gold reaction is 20~30min.

[0041] The present invention also provides a low-phosphorus semi-steel, which is prepared by using any one of the methods in the above technical solutions.

[0042] The solution of the present application is described below through specific embodiments.

[0043] Example 1 60t vanadium-containing molten iron is loaded into an 80t induction furnace, and manganese ore, magnesia sand and iron red are used as vanadium extraction and dephosphorization treatment agents. In terms of weight percentage, the manganese ore used contains 32% Mn, the magnesia sand contains 85% MgO, and the iron red contains 62% TFe, with a particle size of 1-5mm. Manganese ore, magnesia sand and iron red are mixed in a weight ratio of 1:1:8. The molten iron temperature is raised to 1400℃ by an induction furnace, and the mixed vanadium extraction and dephosphorization treatment agent is added in an amount of 50kg / (t iron). The power supply parameters of the induction furnace are adjusted to the insulation gear, and the electromagnetic stirring force is used to promote the slag-iron reaction. The reaction time is controlled at 30min. After the reaction is completed, the vanadium slag is removed, and the low-phosphorus semi-steel is transported to the steelmaking converter for steelmaking. The phosphorus content of the semi-steel is reduced from 0.120% to 0.030%, the dephosphorization rate is 75%, the vanadium content of the semi-steel is reduced from 0.30% to 0.02%, and the vanadium oxidation rate is 93.33%.

[0044] Example 2 40 tons of vanadium-containing molten iron is transferred into a 50t induction furnace, and manganese ore, magnesia and iron oxide are used as vanadium extraction and dephosphorization treatment agents. In terms of weight percentage, the manganese ore contains 30% Mn, the magnesia contains 80% MgO, the iron oxide contains 61% TFe, and the particle size is 1-5mm. The manganese ore, magnesia and iron oxide are mixed in a weight ratio of 2:1.5:6.5. The vanadium-containing molten iron is placed in an induction furnace, the temperature of the molten iron is raised to 1360°C by the induction furnace, and the mixed vanadium extraction and dephosphorization treatment agent is added in an amount of 30kg / (t iron). The power supply parameters of the induction furnace are adjusted to the insulation gear, and the electromagnetic stirring force is used to promote the slag-iron reaction. The reaction time is controlled to 20min. After the reaction is completed, the vanadium slag is removed, and the obtained low-phosphorus semi-steel is transported to the steelmaking converter for steelmaking. The phosphorus content of semi-steel dropped from 0.080% to 0.040%, and the dephosphorization rate was 50%; the vanadium content of semi-steel dropped from 0.32% to 0.03%, and the vanadium oxidation rate was 90.63%.

[0045] Example 3 80 tons of vanadium-containing molten iron are transferred into a 100t induction furnace, and manganese ore, magnesia and iron oxide are used as vanadium extraction and dephosphorization treatment agents. In terms of weight percentage, the manganese ore contains 32% Mn, the magnesia contains 90% MgO, the iron oxide contains 62% TFe, and the particle size is 1-5mm. The manganese ore, magnesia and iron oxide are mixed in a weight ratio of 1.5:1.2:7.8. The vanadium-containing molten iron is placed in an induction furnace, the temperature of the molten iron is raised to 1380°C by the induction furnace, and the mixed vanadium extraction and dephosphorization treatment agent is added in an amount of 40kg / (t iron). The power supply parameters of the induction furnace are adjusted to the insulation gear, and the electromagnetic stirring force is used to promote the slag-iron reaction. The reaction time is controlled to 25min. After the reaction is completed, the vanadium slag is removed, and the obtained low-phosphorus semi-steel is transported to the steelmaking converter for steelmaking. The phosphorus content of semi-steel dropped from 0.075% to 0.035%, and the dephosphorization rate was 53.34%; the vanadium content of semi-steel dropped from 0.35% to 0.04%, and the vanadium oxidation rate was 88.57%.

[0046] After the implementation of the present invention, at least the following beneficial effects are achieved: (1) As the key equipment in this solution, the induction furnace can achieve precise temperature control and rapid heating of semi-steel materials with its unique non-contact heating method, avoiding the problems of element burnout and uneven steel quality that may be caused by traditional heating methods. The induction furnace uses the insulation current to provide electromagnetic stirring force for slag-metal reaction. By accurately controlling the heating temperature and heating time, it provides ideal initial conditions for the subsequent vanadium extraction and dephosphorization process, ensuring that the treatment agent can fully play its role and effectively promote the separation and removal of phosphorus.

[0047] (2) The vanadium extraction and dephosphorization agent can target the chemical characteristics of phosphorus in semi-steel and, through a specific chemical reaction mechanism, efficiently precipitate phosphorus from molten steel and combine it with other components in the slag to form an easily separable compound. This process not only greatly improves the removal efficiency of phosphorus, but also reduces the interference with other beneficial elements during the treatment process, ensuring the stability and purity of the semi-steel components.

[0048] (3) By combining induction furnaces with vanadium extraction and dephosphorization treatment agents, the steel mill not only successfully solved the problem of difficulty in removing phosphorus from vanadium extraction semi-steel, but also significantly improved the quality of semi-steel. After treatment, the phosphorus content of semi-steel was greatly reduced, reaching more stringent usage standards, and better meeting the downstream industry's demand for high-quality steel. At the same time, the improvement of semi-steel quality also means the optimization of product performance, such as the improvement of key indicators such as strength, toughness, and corrosion resistance, thereby enhancing the market adaptability and competitiveness of the product.

[0049] (4) In addition, timely removal of phosphorus from slag is also of great significance for reducing environmental pollution. If phosphorus is discharged directly into the environment without effective treatment, it will pollute water bodies, soil, etc. and affect the ecological balance. However, through the application of vanadium extraction and dephosphorization treatment agents, phosphorus is effectively fixed in the slag, which is convenient for subsequent harmless treatment or resource utilization, realizing a green cycle in the steelmaking production process.

[0050] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0051] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for extracting vanadium and dephosphorizing molten iron, characterized in that: The method comprises heating molten iron with an induction furnace, adding a vanadium extraction and dephosphorization treatment agent, adjusting the power supply parameters of the induction furnace to a heat preservation gear, using the heat preservation gear current to provide an electromagnetic stirring force for slag-metal reaction, removing the vanadium slag after the reaction is completed, obtaining low-phosphorus semi-steel and transporting it to a steelmaking converter for steelmaking.

2. The method for extracting vanadium and dephosphorizing molten iron according to claim 1, characterized in that: The vanadium extraction and dephosphorization treatment agent comprises manganese ore, magnesia and red iron.

3. The method for extracting vanadium and dephosphorizing molten iron according to claim 2, characterized in that: In terms of weight percentage, Mn in the manganese ore is greater than 30%, MgO in the magnesia is greater than 80%, and TFe in the iron oxide is greater than 60%.

4. The method for extracting vanadium and dephosphorizing molten iron according to claim 2, characterized in that: The particle size range of the manganese ore, magnesia and red iron is 1-5 mm.

5. The method for extracting vanadium and dephosphorizing molten iron according to claim 2, characterized in that: The manganese ore, magnesia and red iron ore are fully mixed in a weight ratio of 1-2:1-1.5:6.5-8.

6. The method for extracting vanadium and dephosphorizing molten iron according to claim 1, characterized in that: Adjusting the power supply parameter of the induction furnace to the insulation gear includes determining whether the induction furnace is in the insulation gear by detecting the working state of the induction furnace, wherein the working state includes real-time temperature and / or heating speed.

7. The method for extracting vanadium and dephosphorizing molten iron according to claim 1, characterized in that: The heating includes heating to 1360-1400°C.

8. The method for extracting vanadium and dephosphorizing molten iron according to claim 1, characterized in that: The amount of the vanadium extraction and dephosphorization agent added is 30-50 kg / (t iron).

9. The method for extracting vanadium and dephosphorizing molten iron according to claim 1, characterized in that: The reaction time of the slag-gold reaction is 20 to 30 minutes.

10. A low-phosphorus semi-steel, characterized in that: The method is prepared by any one of claims 1 to 9.

Citation Information

Cited By

  • Smelting method based on large-tonnage double-frequency induction melting electric furnace

    CN119803076A

  • A smelting method based on a large-tonnage double-frequency induction smelting electric furnace