Chemical copper plating solution as well as preparation method and application thereof

By using hypophosphite and aminoborane as a combination of reducing agents and combining with other additives, the stability and deposition rate of electroless copper plating solution are improved, and the environmental risk of formaldehyde and insufficient binding force of the plating in the prior art are solved, so as to achieve Efficient and environmentally friendly copper plating process.

CN118957554AInactive Publication Date: 2024-11-15DONGFANG HUANSHENG PHOTOVOLTAIC (JIANGSU) CO LTD

Patent Information

Application Number
CN202411047251.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The formaldehyde reducing agent commonly used in the existing electroless copper plating process has environmental risks, insufficient stability, slow deposition rate, and poor binding capacity between the plating and the substrate, making it difficult to meet the dual needs of environmental protection and industrial applications.

Method used

Using hypophosphite and aminoborane as a combination of reducing agents, combined with complexing agents, stabilizers, accelerators and wetting agents, an electroless copper plating solution is designed to improve copper plating by carefully controlling the pH value and the order of raw material addition. The stability and deposition rate of the liquid enhance the binding force between the plating and the substrate.

Benefits of technology

It significantly reduces environmental pollution, improves the efficiency and quality of the copper plating process, ensures the uniformity and long-term stability of the plating, and meets the needs of environmental protection and industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004975327710000111
    Figure BDA0004975327710000111
  • Figure BDA0004975327710000121
    Figure BDA0004975327710000121
  • Figure BDA0004975327710000131
    Figure BDA0004975327710000131
Patent Text Reader

Abstract

The invention provides a chemical copper plating solution and a preparation method and application thereof, and particularly relates to the technical field of solar cell preparation. The chemical copper plating solution provided by the invention comprises copper salt, a reducing agent, a complexing agent, a stabilizing agent, an accelerating agent and a wetting agent, the reducing agent comprises hypophosphorous acid and amino borane. According to the chemical copper plating solution provided by the invention, hypophosphorous acid is adopted as a main reducing agent, and amino borane is supplemented as an auxiliary reducing agent, so that the pollution to the environment is remarkably reduced by the combination. The synergistic effect of the two reducing agents is remarkable, and the reducing capacity is effectively improved, so that the deposition rate of chemical copper plating is increased. In addition, by adding a small amount of well-designed stabilizer and accelerator, the stability of the chemical copper plating solution is further optimized, and the binding force of a plating layer and a base material is remarkably enhanced. The innovative formula not only improves the efficiency and quality of the copper plating process, but also meets the dual requirements of environmental protection and industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cell preparation, and in particular to a chemical copper plating solution and a preparation method and application thereof. Background Art

[0002] Electroplating technology is an advanced non-contact electrode manufacturing process that can not only perfectly replace traditional silver paste, but also has excellent performance and can significantly reduce production costs. In the process of manufacturing electroplated solar cells, a layer of metal is first deposited on the silicon substrate as a seed layer, and then copper is electroplated on it to form a conductive layer, and finally covered with a layer of metal as a protective layer to complete the preparation of electroplated solar cells.

[0003] In the copper plating process, you can choose between electroplating copper and chemical copper plating. As a self-catalytic process, chemical plating has the advantages of simple operation and easy control of reaction conditions compared to electroplating. Chemical plating stands out for its low porosity, uniform thickness, good corrosion resistance and excellent wear resistance, and is particularly suitable for comprehensive coverage of parts with complex shapes. Considering the specific material and structure of monocrystalline silicon solar cells, chemical copper plating is undoubtedly an ideal choice.

[0004] However, although formaldehyde, a commonly used reducing agent in the current chemical copper plating process, has significant reduction effects and low costs, it poses serious environmental risks. In addition, the chemical plating solution itself is not stable enough, the deposition rate is slow, and the bonding strength with the substrate is not satisfactory.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] One of the purposes of the present invention is to provide a chemical copper plating solution, aiming to solve at least one of the above-mentioned technical problems in the prior art.

[0007] A second object of the present invention is to provide a method for preparing a chemical copper plating solution.

[0008] A third object of the present invention is to provide an application of a chemical copper plating solution.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] The first aspect of the present invention provides a chemical copper plating solution comprising a copper salt, a reducing agent, a complexing agent, a stabilizer, an accelerator and a wetting agent.

[0011] The reducing agent includes hypophosphorous acid and aminoborane.

[0012] Furthermore, the mass ratio of the hypophosphorous acid to the aminoborane is 10-30:0.5-3.

[0013] Furthermore, the copper salt includes at least one of copper sulfate, copper chloride, copper nitrate and copper acetate.

[0014] Preferably, the complexing agent includes at least one of potassium sodium tartrate, sodium citrate, disodium ethylenediaminetetraacetate, sodium gluconate, triethanolamine and tetrahydroxypropylethylenediamine.

[0015] Preferably, the stabilizer includes at least one of potassium ferrocyanide, Tween-60, potassium perfluorooctane sulfonate, 2,2'-bipyridyl, sodium silicate, sodium hexafluorosilicate and sodium sulfite.

[0016] Preferably, the accelerator comprises at least one of 2-mercaptobenzothiazole, polyvinylpyrrolidone, L-malic acid, 2-amino-6-hydroxypurine and 6-aminopurine.

[0017] Preferably, the wetting agent includes at least one of polyoxyethylene fatty alcohol ether, alkylphenol polyoxyethylene ether, fatty acid polyoxyethylene ester and polyoxyethylene alkylamine.

[0018] Furthermore, the chemical copper plating solution comprises, per unit volume, 20 to 50 parts of copper salt, 10 to 30 parts of reducing agent, 15 to 30 parts of complexing agent, 1 to 10 parts of stabilizer, 3 to 20 parts of accelerator and 5 to 10 parts of wetting agent in parts by weight.

[0019] The second aspect of the present invention provides a method for preparing the chemical copper plating solution, wherein a complexing agent, a stabilizer, an accelerator, a wetting agent and a reducing agent are sequentially added to a copper salt solution to obtain the chemical copper plating solution.

[0020] Furthermore, after adding the complexing agent, the pH of the solution is adjusted to 7.0-8.0.

[0021] Preferably, after adding the wetting agent, the pH of the solution is then adjusted to 11.0-12.0.

[0022] The third aspect of the present invention provides the use of the chemical copper plating solution in copper plating of solar cells.

[0023] Furthermore, the process of copper plating the solar cell includes:

[0024] The solar cell silicon substrate with double-sided nickel plating is placed in a chemical copper plating solution for chemical copper plating to obtain a copper electrode.

[0025] Furthermore, the temperature of the chemical copper plating is 40°C to 50°C.

[0026] Preferably, the pH of the chemical copper plating is 11.0-12.0.

[0027] Furthermore, the solar cell copper plating process also includes cleaning and drying steps after chemical copper plating;

[0028] Preferably, deionized water is used for the cleaning;

[0029] Preferably, the drying temperature is 50°C to 60°C.

[0030] Compared with the prior art, the present invention has at least the following beneficial effects:

[0031] The chemical copper plating solution provided by the present invention adopts hypophosphorous acid as the main reducing agent and aminoborane as the auxiliary reducing agent. This combination significantly reduces the pollution to the environment. The synergistic effect of the two reducing agents is significant, and the reducing ability is effectively improved, thereby accelerating the deposition rate of chemical copper plating. In addition, by adding a small amount of carefully designed stabilizers and accelerators, the stability of the chemical copper plating solution is further optimized, and the bonding force between the coating and the substrate is significantly enhanced. This innovative formula not only improves the efficiency and quality of the copper plating process, but also meets the dual needs of environmental protection and industrial application.

[0032] The method for preparing the chemical copper plating solution provided by the present invention significantly improves the activity of the chemical reaction by a well-designed raw material addition sequence. This strategy not only enhances the stability of the chemical copper plating solution, but also ensures the quality of the chemical copper plating solution. The process flow of the preparation method is concise and clear, easy to operate, very suitable for large-scale industrial production needs, and can maximize production efficiency while ensuring product quality.

[0033] The application of the chemical copper plating solution provided by the present invention, in view of the advantages of the above chemical copper plating solution, makes the obtained copper plating layer have good uniformity and higher bonding strength, thereby improving the photoelectric conversion efficiency of the solar cell, and at the same time the good bonding strength ensures the long-term stability of the solar cell. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0035] Hereinafter, the terms "including", "having" and their cognates, which may be used in various embodiments of the present invention, are intended only to indicate specific features, numbers, steps, operations, elements, components or combinations of the foregoing items, and should not be understood as first excluding the existence of one or more other features, numbers, steps, operations, elements, components or combinations of the foregoing items or adding the possibility of one or more features, numbers, steps, operations, elements, components or combinations of the foregoing items.

[0036] The first aspect of the present invention provides a chemical copper plating solution comprising a copper salt, a reducing agent, a complexing agent, a stabilizer, an accelerator and a wetting agent.

[0037] The reducing agent includes hypophosphorous acid and aminoborane.

[0038] The chemical copper plating solution provided by the present invention adopts hypophosphorous acid as the main reducing agent and aminoborane as the auxiliary reducing agent. This combination significantly reduces the pollution to the environment. The synergistic effect of the two reducing agents is significant, and the reducing ability is effectively improved, thereby accelerating the deposition rate of chemical copper plating. In addition, by adding a small amount of carefully designed stabilizers and accelerators, the stability of the chemical copper plating solution is further optimized, and the bonding force between the coating and the substrate is significantly enhanced. This innovative formula not only improves the efficiency and quality of the copper plating process, but also meets the dual needs of environmental protection and industrial application.

[0039] Specifically, in the formula of the above-mentioned chemical copper plating solution, each component has a specific function to ensure the efficiency and quality of the chemical copper plating process: sodium hypophosphite and aminoborane are used as compound reducing agents, and their main function is to reduce copper ions to copper metal to form a copper layer deposited on the substrate. Aminoborane has a strong reducing ability, a fast deposition rate, and good coating performance, but if it is added in too much amount, it will cause the plating solution to decompose easily, so it needs to be compounded with sodium hypophosphite and used together with a complexing agent to obtain a higher copper deposition effect. Complexing agents such as potassium sodium tartrate, sodium citrate, etc. are used to form stable complexes with copper ions to control the activity and reactivity of copper ions. This helps to prevent the uncontrolled deposition of copper ions and ensure the uniformity and controllability of the coating. Stabilizers such as potassium ferrocyanide, Tween-60, etc. are used to inhibit side reactions in chemical copper plating solutions, such as hydrolysis and oxidation of copper ions. Stabilizers help maintain the long-term stability of the plating solution and prevent coating quality problems caused by instability. Accelerators such as 2-mercaptobenzothiazole and polyvinylpyrrolidone are used to speed up the reaction rate of chemical copper plating, thereby shortening the copper plating time and improving production efficiency. Accelerators can also help improve the crystallization and surface properties of the coating. Wetting agents include polyoxyethylene fatty alcohol ethers, alkylphenol polyoxyethylene ethers, etc. Their function is to improve the spreadability of the plating solution on the substrate surface and increase the contact area between the plating solution and the substrate, thereby improving the uniformity and adhesion of the coating.

[0040] Furthermore, the mass ratio of the hypophosphorous acid to the aminoborane is 10-30:0.5-3.

[0041] Typically, but not limiting, the mass ratio of hypophosphorous acid to aminoborane can be 10:0.5, 11:0.6, 12:0.7, 13:0.8, 14:0.9, 15:1, 16:1.1, 17:1.2, 18:1.3, 19:1.4, 20:1.5, 21:1.6, 22:1.7, 23:1.8, 24:1.9, 25:2, 26:2.1, 27:2.2, 28:2.3, 29:2.4 or 30:2.5, or any ratio within the range of 10:0.5 to 30:0.

[0042] Furthermore, the copper salt includes at least one of copper sulfate, copper chloride, copper nitrate and copper acetate.

[0043] Preferably, the complexing agent includes at least one of potassium sodium tartrate, sodium citrate, disodium ethylenediaminetetraacetate, sodium gluconate, triethanolamine and tetrahydroxypropylethylenediamine.

[0044] Preferably, the stabilizer includes at least one of potassium ferrocyanide, Tween-60, potassium perfluorooctane sulfonate, 2,2'-bipyridyl, sodium silicate, sodium hexafluorosilicate and sodium sulfite.

[0045] Preferably, the accelerator comprises at least one of 2-mercaptobenzothiazole, polyvinylpyrrolidone, L-malic acid, 2-amino-6-hydroxypurine and 6-aminopurine.

[0046] Preferably, the wetting agent includes at least one of polyoxyethylene fatty alcohol ether, alkylphenol polyoxyethylene ether, fatty acid polyoxyethylene ester and polyoxyethylene alkylamine.

[0047] Furthermore, the chemical copper plating solution comprises, per unit volume, 20 to 50 parts of copper salt, 10 to 30 parts of reducing agent, 15 to 30 parts of complexing agent, 1 to 10 parts of stabilizer, 3 to 20 parts of accelerator and 5 to 10 parts of wetting agent in parts by weight.

[0048] Typically but not limiting, each volume of chemical copper plating solution may specifically include the following components by weight: copper salt: 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts or 50 parts, or any value within the range of 20 to 50 parts; reducing agent: 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, 22 parts or 30 parts, or any value within the range of 10 to 30 parts; complexing agent: 15 parts, 17 parts, 20 parts, 22 parts or 30 parts, or any value within the range of 10 to 30 parts; The amount of the stabilizer can be 1 part, 3 parts, 5 parts, 7 parts or 10 parts, or any value within the range of 1 part to 10 parts; the accelerator can be 3 parts, 6 parts, 9 parts, 12 parts, 15 parts, 18 parts or 20 parts, or any value within the range of 3 parts to 20 parts; the wetting agent can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts, or any value within the range of 5 parts to 10 parts.

[0049] The second aspect of the present invention provides a method for preparing the chemical copper plating solution, wherein a complexing agent, a stabilizer, an accelerator, a wetting agent and a reducing agent are sequentially added to a copper salt solution to obtain the chemical copper plating solution.

[0050] The method for preparing the chemical copper plating solution provided by the present invention significantly improves the activity of the chemical reaction by a well-designed raw material addition sequence. This strategy not only enhances the stability of the chemical copper plating solution, but also ensures the quality of the chemical copper plating solution. The process flow of the preparation method is concise and clear, easy to operate, very suitable for large-scale industrial production needs, and can maximize production efficiency while ensuring product quality.

[0051] Furthermore, after adding the complexing agent, the pH of the solution is adjusted to 7.0-8.0 to prevent the formation of copper hydroxide precipitation and ensure that the copper ions exist in the form of complex ions.

[0052] The present invention does not specifically limit the reagent used for adjusting the pH, and any reagent that does not react with the raw materials of the chemical copper plating solution and does not affect the performance of the chemical copper plating solution can be used.

[0053] Preferably, after adding the wetting agent, the pH of the solution is then adjusted to 11.0-12.0.

[0054] The pH of the solution is controlled at 11.0-12.0 after adding the wetting agent and before adding the reducing agent. This is because the higher the pH, the stronger the reducing effect of sodium hypophosphite and the faster the copper deposition rate. However, if the pH is higher than 12.0, the solution will lose stability and the coating will become rough or uneven.

[0055] The third aspect of the present invention provides the use of the chemical copper plating solution in copper plating of solar cells.

[0056] The application of the chemical copper plating solution provided by the present invention, in view of the advantages of the above chemical copper plating solution, makes the obtained copper plating layer have good uniformity and higher bonding strength, thereby improving the photoelectric conversion efficiency of the solar cell, and at the same time the good bonding strength ensures the long-term stability of the solar cell.

[0057] Furthermore, the process of copper plating the solar cell includes:

[0058] The solar cell silicon substrate with double-sided nickel plating is placed in a chemical copper plating solution for chemical copper plating to obtain a copper electrode.

[0059] Furthermore, the temperature of the chemical copper plating is 40°C to 50°C.

[0060] Typically but not limiting, the temperature setting during the chemical copper plating process can be precisely set to a specific value, for example, it can be set to 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 49°C or 50°C. At the same time, this temperature range also allows adjustment to any value between 40°C and 50°C to adapt to different process requirements and operating conditions.

[0061] Preferably, the pH of the chemical copper plating is 11.0-12.0.

[0062] The pH of chemical copper plating is controlled at 11.0-12.0 because under this condition, sodium hypophosphite is more effective in reducing copper ions and has higher activity. Within the above pH range, the reaction rate can be optimized to obtain the desired coating thickness and quality.

[0063] Typically but not limiting, the pH value in the chemical copper plating process can be accurate to one decimal place, for example, it can be set to 11.0, 11.1, 11.2, 11.3, 11.4, 11.5, 11.6, 11.7, 11.8 or 12.0. At the same time, the pH value can also be any value within the range of 11.0 to 12.0 to adapt to different chemical copper plating conditions and improve the quality of the coating.

[0064] Furthermore, the solar cell copper plating process also includes cleaning and drying steps after chemical copper plating;

[0065] Preferably, deionized water is used for the cleaning;

[0066] Preferably, the drying temperature is 50°C to 60°C.

[0067] Typically but not limiting, the temperature during the drying process can be set to 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C or 60°C, which are all feasible options. In addition, the drying temperature can also be any value within the range of 50°C to 60°C.

[0068] The present invention is further described below by specific examples and comparative examples, but it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form. The raw materials used in the examples and comparative examples of the present invention, if no specific conditions are specified, are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0069] The preparation method of aminoborane used in the examples and comparative examples is:

[0070] 1 mol of ammonium fluoroborate and 1 mol of sodium borohydride are placed in a reactor with a reflux device containing 250 mL of 1,4-dioxane solvent to obtain a mixed solution. Then, the mixture is heated and stirred for 2 to 5 hours, and the mixed solution is filtered to obtain a clear and transparent solution; the clear solution is rotary evaporated to obtain a white sample, which is aminoborane.

[0071] Example 1

[0072] This embodiment provides a chemical copper plating solution, and the preparation method is as follows:

[0073] Take 35g of copper chloride and dissolve it in deionized water, stir until it is completely dissolved, add 22g of potassium sodium tartrate, mix and stir well, and adjust the pH to 7.5 with alkali; then continue to add 5mg of sodium silicate, 11mg of polyvinyl pyrrolidone, and 12mg of polyoxyethylene fatty alcohol ether, adjust the volume with deionized water, and then adjust the pH to 11.5 with alkali, finally add 20g of sodium hypophosphite and 2g of aminoborane and stir well, and finally add deionized water to make up to 1L to obtain a chemical copper plating solution.

[0074] Example 2

[0075] This embodiment provides a chemical copper plating solution, and the preparation method is as follows:

[0076] Take 40g of copper sulfate and dissolve it in deionized water, stir until it is completely dissolved, add 26g of sodium citrate, mix and stir thoroughly, and adjust the pH to 7.2 with alkali; then continue to add 6mg of sodium sulfite, 15mg of 2-mercaptobenzothiazole, and 7mg of alkylphenol polyoxyethylene ether, adjust the volume with deionized water, and then adjust the pH to 11 with alkali, finally add 15g of sodium hypophosphite and 1g of aminoborane and stir thoroughly, and finally add deionized water to make the volume to 1L to obtain a chemical copper plating solution.

[0077] Example 3

[0078] This embodiment provides a chemical copper plating solution, and the preparation method is as follows:

[0079] Take 25g of copper nitrate and dissolve it in deionized water, stir until it is completely dissolved, add 20g of sodium gluconate, mix and stir thoroughly, and adjust the pH to 7.8 with alkali; then continue to add 7mg of sodium hexafluorosilicate, 10mg of 6-aminopurine, and 7mg of fatty acid polyoxyethylene ester, adjust the volume with deionized water, and then adjust the pH to 11 with alkali, finally add 21g of sodium hypophosphite and 2g of aminoborane and stir thoroughly, and finally add deionized water to make the volume to 1L to obtain a chemical copper plating solution.

[0080] Example 4

[0081] This embodiment provides a chemical copper plating solution, and the preparation method is as follows:

[0082] Take 35g of copper chloride and dissolve it in deionized water, stir until it is completely dissolved, add 11g of triethanolamine and 11g of disodium ethylenediaminetetraacetate, mix and stir well, and adjust the pH to 7.5 with alkali; then continue to add 5mg of sodium silicate, 5mg of polyvinyl pyrrolidone, 6mg of L-malic acid, 6mg of polyoxyethylene fatty alcohol ether, and 6mg of polyoxyethylene alkylamine, adjust the volume with deionized water, and then adjust the pH to 11.5 with alkali, finally add 28g of sodium hypophosphite and 1g of aminoborane and stir well, and finally add deionized water to make the volume to 1L to obtain a chemical copper plating solution.

[0083] Example 5

[0084] This embodiment provides a chemical copper plating solution. The difference from Embodiment 1 is that 10 g of sodium hypophosphite and 0.5 g of aminoborane are used. The remaining raw materials and methods are the same as those in Embodiment 1 and will not be described again.

[0085] Example 6

[0086] This embodiment provides a chemical copper plating solution. The difference from Embodiment 1 is that 27 g of sodium hypophosphite and 3 g of aminoborane are used. The remaining raw materials and methods are the same as those in Embodiment 1 and will not be described again.

[0087] Example 7

[0088] This embodiment provides a chemical copper plating solution. The difference from Embodiment 1 is that 10 g of sodium hypophosphite and 10 g of aminoborane are used. The remaining raw materials and methods are the same as those in Embodiment 1 and will not be described again.

[0089] Example 8

[0090] This embodiment provides a chemical copper plating solution. The difference from Embodiment 1 is that 20 g of sodium hypophosphite and 10 g of aminoborane are used. The remaining raw materials and methods are the same as those in Embodiment 1 and will not be described again.

[0091] Example 9

[0092] This embodiment provides a chemical copper plating solution. The difference from Embodiment 1 is that the amount of polyvinyl pyrrolidone added is 2 mg. The remaining raw materials and methods are the same as those in Embodiment 1 and will not be described again.

[0093] Example 10

[0094] This embodiment provides a chemical copper plating solution. The difference from Embodiment 1 is that the amount of polyvinyl pyrrolidone added is 22 mg. The remaining raw materials and methods are the same as those in Embodiment 1 and will not be described again.

[0095] Embodiment 11

[0096] This embodiment provides a chemical copper plating solution. The difference from Embodiment 1 is that the amount of polyoxyethylene fatty alcohol ether added is 3 mg, and the remaining raw materials and methods are the same as those in Embodiment 1, which will not be described again.

[0097] Example 12

[0098] This embodiment provides a chemical copper plating solution. The difference from Embodiment 1 is that the amount of polyoxyethylene fatty alcohol ether added is 13 mg, and the remaining raw materials and methods are the same as those in Embodiment 1, which will not be described again.

[0099] Comparative Example 1

[0100] This comparative example provides a chemical copper plating solution. The difference from Example 1 is that aminoborane is not added. The remaining raw materials and methods are the same as those in Example 1 and will not be described again.

[0101] Comparative Example 2

[0102] This comparative example provides a chemical copper plating solution. The difference from comparative example 1 is that formaldehyde is used to replace sodium hypophosphite. The remaining raw materials and methods are the same as those in comparative example 1 and will not be repeated here.

[0103] Comparative Example 3

[0104] This comparative example provides a chemical copper plating solution. The difference from Example 1 is that polyvinyl pyrrolidone is not added. The remaining raw materials and methods are the same as those in Example 1 and will not be described again.

[0105] Comparative Example 4

[0106] This comparative example provides a chemical copper plating solution. The difference from Example 1 is that no polyoxyethylene fatty alcohol ether is added. The remaining raw materials and methods are the same as those in Example 1 and will not be described again.

[0107] Test Example 1

[0108] The chemical copper plating solutions obtained in the examples and comparative examples were placed in a constant temperature water bath at 75° C. and heated for 1 hour. The changes were observed and recorded in Table 1.

[0109] Test Example 2

[0110] The solar cell silicon substrate with double-sided nickel plating was immersed in the chemical copper plating solution obtained in the embodiment and the comparative example, the temperature was controlled at 45°C, the pH was 11.5, and the chemical copper plating process was carried out. The chemical copper plating time was 1 hour, and the deposition rate was tested during the process.

[0111] Deposition rate test: Determination of chemical copper deposition rate by weight gain method:

[0112] v = (m1-m0) × 10000 / (ρSt);

[0113] v is the deposition rate, in μm / h; m1 is the mass of the silicon substrate after double-sided copper plating, in g; m0 is the mass of the silicon substrate before double-sided nickel plating, in g; ρ is the density of copper, which is 8.9 g / cm 3 ; S is the area of ​​the copper grid, in cm 2 ; t is the chemical copper plating deposition time, the unit is h, and the obtained data are shown in Table 1.

[0114] It should be noted that the stability of the chemical copper plating solution is determined by observing whether the plating solution changes during the reaction process. A stable chemical copper plating solution maintains its clarity and transparency throughout the copper plating process.

[0115] If the plating solution remains clear in the plating tank and there is no copper deposit at the bottom, it indicates that the plating solution has good stability. On the contrary, if copper deposits are found at the bottom of the plating tank, it means that the plating solution is unstable.

[0116] Table 1

[0117]

[0118]

[0119] As can be seen from Table 1, when hypophosphorous acid is used as the main reducing agent and aminoborane is used as the auxiliary reducing agent, the two are matched in a suitable ratio and the synergistic effect is significant, which can effectively improve the reducing ability and accelerate the deposition rate of chemical copper plating; and with the assistance of additives such as stabilizers and complexing agents, it helps to maintain the stability of the plating solution and increase the service life of the plating solution.

[0120] Test Example 3

[0121] The double-sided copper-plated solar cell obtained in Test Example 2 was subjected to a coating bonding strength test. The main grid and PAD points of the metal copper grid lines on the front and back of the crystalline silicon solar cell were covered with low-temperature solder tape, assisted by a small amount of medium-temperature solder paste, and soldered at 180°C. The welding tension at 12 PAD points was tested with a tensile gauge, and the average value was taken (all points ≥0.8N were qualified). The obtained data were recorded in Table 2.

[0122] Table 2

[0123]

[0124] As can be seen from Table 2, hypophosphorous acid was used as the main reducing agent, and aminoborane was used as the auxiliary reducing agent. The two reducing agents had a good synergistic effect. This synergistic effect not only increased the deposition rate of the coating, but also improved the adhesion of the coating. The welding tensile force of the front and back grid lines tested under low temperature conditions was higher than that of using a single reducing agent, indicating that this plating solution system helps to improve the adhesion between the coating and the silicon substrate of the solar cell.

[0125] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A chemical copper plating solution, It is characterized in that Includes copper salts, reducing agents, complexing agents, stabilizers, accelerators and wetting agents; The reducing agent includes hypophosphorous acid and aminoborane.

2. The chemical copper plating solution according to claim 1, It is characterized in that The mass ratio of the hypophosphorous acid to the aminoborane is 10-30:0.5-3.

3. The chemical copper plating solution according to claim 1, It is characterized in that The copper salt includes at least one of copper sulfate, copper chloride, copper nitrate and copper acetate; Preferably, the complexing agent includes at least one of potassium sodium tartrate, sodium citrate, disodium ethylenediaminetetraacetate, sodium gluconate, triethanolamine and tetrahydroxypropylethylenediamine; Preferably, the stabilizer includes at least one of potassium ferrocyanide, Tween-60, potassium perfluorooctane sulfonate, 2,2'-bipyridyl, sodium silicate, sodium hexafluorosilicate and sodium sulfite; Preferably, the accelerator comprises at least one of 2-mercaptobenzothiazole, polyvinylpyrrolidone, L-malic acid, 2-amino-6-hydroxypurine and 6-aminopurine; Preferably, the wetting agent includes at least one of polyoxyethylene fatty alcohol ether, alkylphenol polyoxyethylene ether, fatty acid polyoxyethylene ester and polyoxyethylene alkylamine.

4. The chemical copper plating solution according to claim 1, It is characterized in that Each unit volume includes, by weight, 20 to 50 parts of copper salt, 10 to 30 parts of reducing agent, 15 to 30 parts of complexing agent, 1 to 10 parts of stabilizer, 3 to 20 parts of accelerator and 5 to 10 parts of wetting agent.

5. A method for preparing the chemical copper plating solution according to any one of claims 1 to 4, It is characterized in that A complexing agent, a stabilizer, an accelerator, a wetting agent and a reducing agent are sequentially added into a copper salt solution to obtain the chemical copper plating solution.

6. The preparation method according to claim 5, It is characterized in that After adding the complexing agent, the pH of the solution is then adjusted to 7.0-8.0; Preferably, after adding the wetting agent, the pH of the solution is then adjusted to 11.0-12.

0.

7. Use of the chemical copper plating solution according to any one of claims 1 to 4 in copper plating of solar cells.

8. The use according to claim 7, It is characterized in that The process of copper plating of solar cells comprises: The solar cell silicon substrate with double-sided nickel plating is placed in a chemical copper plating solution for chemical copper plating to obtain a copper electrode.

9. The use according to claim 8, It is characterized in that The temperature of the chemical copper plating is 40°C to 50°C; Preferably, the pH of the chemical copper plating is 11.0-12.

0.

10. The use according to claim 8, It is characterized in that Also included are cleaning and drying steps after chemical copper plating; Preferably, deionized water is used for the cleaning; Preferably, the drying temperature is 50°C to 60°C.

Citation Information

Patent Citations

  • Method for preparing front electrodes of solar cells

    CN101562217A

  • Chemical copper plating liquid and chemical copper plating method

    CN102877046A

  • Positive electrode grid line solar cell, solar cell and method for manufacturing positive electrode grid line of solar cell and solar cell

    CN106531818A

  • Electroless copper plating solution for heterojunction solar cell and preparation method thereof

    CN111962051A

  • Double-complexing-system low-stress electroless copper plating solution and preparation method and application thereof

    CN113897600A

Cited By

  • Photovoltaic conductive method and preparation of electroplating reduction pretreatment agent