Deposition aid for spray deposition of zinc-aluminum-magnesium plating layer, spray material and preparation method
By using a deposition agent such as silver nitrate to activate zinc-aluminum magnesium powder, the problem of forming a uniform coating with the steel surface is solved, the density and high binding force of zinc-aluminum magnesium plating are achieved, and the coating is improved. Environmental protection and corrosion resistance.
Patent Information
- Application Number
- CN202411051429.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
Due to the chemical reaction between zinc-aluminum magnesium powder and steel, it is difficult to form a uniform and dense coating. The existing jet material formula for jet deposited zinc plating lacks reference value, and the surface activity and electrode potential of zinc-aluminum magnesium powder are as good as traditional. The zinc coating materials are different, which makes it difficult to deposition.
Use a deposition agent including silver nitrate, titanium dioxide, nickel sulfamate, TX-10, sodium phosphite, stannous sulfate, sodium molybdate, sodium hydroxide, weak alkali and other components to form Group B evenly by stirring Component C, combined with zinc-aluminum magnesium powder, form spray material that sprays deposited galvanized aluminum-aluminum magnesium plating, promotes activation and adhesion of zinc-aluminum magnesium powder, and forms a uniform and dense zinc-aluminum magnesium plating layer.
Under the action of the deposition agent, zinc, aluminum, magnesium powder forms a uniform and dense coating on the surface of steel parts, enhancing the binding force with the substrate, improving the added value, environmental protection and corrosion resistance of the coating, reducing weight, and improving the efficiency of the application .
Smart Images

Figure CN118957561A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of spray-deposited zinc-aluminum-magnesium coatings, and in particular relates to a deposition aid, a spray material and a preparation method for spray-deposited zinc-aluminum-magnesium coatings. Background Art
[0002] With the development of engineering technology, the requirements of modern anti-corrosion technology are constantly increasing. Now is an era of equal emphasis on science and technology and environmental protection. We should not only pursue superior corrosion resistance but also better environmental performance. Zinc-aluminum-magnesium coating has excellent performance and can greatly improve the corrosion resistance of steel parts. Even in corrosive media such as acid and alkali, it can maintain stability and extend the service life of steel parts. In addition, the wear resistance and high temperature resistance of steel parts are also greatly improved. Zinc-aluminum-magnesium coating also has the characteristics of lightweight. Compared with other coatings, it can reduce the weight of steel parts under the condition of the same thickness and improve the efficiency of material use. Zinc-aluminum-magnesium coating can give steel parts a good appearance and decorative effect, and improve the added value of steel parts. The most important point is that zinc-aluminum-magnesium coating has good environmental performance and extremely light pollution to the environment, which is completely in line with the development and use direction of coatings today.
[0003] However, due to the chemical properties of zinc-aluminum-magnesium powder, the zinc-aluminum-magnesium powder will react chemically with steel, which is not conducive to forming a uniform and dense coating. In addition, there is a large difference in chemical affinity between zinc-aluminum-magnesium powder and steel. These conditions make it difficult for zinc-aluminum-magnesium powder to form a uniform coating on the surface of steel. In addition, the surface activity, electrode potential and chemical properties of zinc-aluminum-magnesium powder are completely different from those of the raw material zinc powder of traditional zinc coating, which results in the existing developed spray-deposited zinc coating spray material formula having no reference value. Moreover, the chemical composition, surfactant and electrode potential of zinc powder, aluminum powder and magnesium powder in zinc-aluminum-magnesium powder are quite different. Therefore, when spraying and depositing the coating, it is difficult to effectively deposit on the surface of steel parts due to the difficulty in controlling the surface activation of the raw material powder. Therefore, it has become inevitable to develop a spray material suitable for zinc-aluminum-magnesium powder for use in the preparation of spray-deposited zinc-aluminum-magnesium coating. Summary of the invention
[0004] In view of the shortcomings of the above-mentioned prior art, the present invention proposes a deposition aid, a spray material and a preparation method for spray-deposited zinc-aluminum-magnesium coating. Under the promotion of the deposition aid, zinc-aluminum-magnesium powder will generate an oxide film, which improves the activity, adhesion and stability of the zinc-aluminum-magnesium powder, so that the zinc-aluminum-magnesium powder can form a uniform, dense and firm zinc-aluminum-magnesium coating on the steel substrate.
[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a deposition aid for spray-deposited zinc-aluminum-magnesium coating includes component B and component C; component B includes silver nitrate, titanium dioxide, nickel sulfamate, TX-10 and water; component C includes sodium hypophosphite, stannous sulfate, sodium molybdate, sodium hydroxide, weak base and water.
[0006] As a preferred embodiment of the present invention, the mass percentage of component B in the deposition aid is 40% to 50%, and the mass percentage of component C is 50% to 60%.
[0007] More preferably, the mass percentage of the B component is 45% to 50%, and the mass percentage of the C component is 50% to 55%.
[0008] As a preferred embodiment of the present invention, the B component includes the following components in percentage by mass: 7% to 10% silver nitrate, 4% to 7% titanium dioxide, 4% to 9% nickel sulfamate, 2% to 5% TX-10 and the balance water.
[0009] As a preferred embodiment of the present invention, the C component includes the following components in percentage by mass: 5% to 8% sodium hypophosphite, 8% to 20% stannous sulfate, 1.5% to 3% sodium molybdate, 1% to 2.5% sodium hydroxide, 1% to 2.5% weak base and balance water.
[0010] As a preferred embodiment of the present invention, the weak base is one or more of aluminum hydroxide, copper hydroxide, ferrous hydroxide, and ammonia water.
[0011] The present invention also claims to protect a spray material for spray-deposited zinc-aluminum-magnesium coating, comprising the A component and a deposition aid for spray-deposited zinc-aluminum-magnesium coating; the A component comprises zinc-aluminum-magnesium powder and a spray-deposited medium.
[0012] As a preferred embodiment of the present invention, the spray material for spray-deposited zinc-aluminum-magnesium coating comprises: component A and a deposition aid; the mass ratio of component A to the deposition aid is 201:(10-20).
[0013] As a preferred embodiment of the present invention, the spray deposition medium is one or two of zirconium beads, alumina beads, and steel beads; the mass ratio of the spray deposition medium to the zinc-aluminum-magnesium powder is (165-200):1.
[0014] As a preferred embodiment of the present invention, the method for preparing the spray material for spray-depositing zinc-aluminum-magnesium coating comprises the following steps:
[0015] (1) silver nitrate and nickel sulfamate are placed in water and stirred, and titanium dioxide and TX-10 are added during the stirring process until the mixture is stirred evenly to obtain component B;
[0016] (2) adding stannous sulfate into water and stirring, adding sodium hypophosphite and sodium molybdate during the stirring process, and finally adding sodium hydroxide and a weak base until the stirring is uniform to obtain component C;
[0017] (3) Components B and C are stirred evenly, and after reacting for 90 seconds, component A is added to obtain a spray material for spray-deposited zinc-aluminum-magnesium coating.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) Under the action of the deposition aid of the spray-deposited zinc-aluminum-magnesium coating, the zinc-aluminum-magnesium powder is adsorbed on the surface of the steel workpiece in the liquid medium of the deposition aid, and a dense and uniform zinc-aluminum-magnesium coating is formed through the spray-deposited coating preparation process. The bonding between the zinc-aluminum-magnesium coating and the substrate is enhanced, which greatly reduces the probability of the zinc-aluminum-magnesium powder being peeled off by the spray-deposited medium. Compared with zinc-coated parts, zinc-aluminum-magnesium coated steel parts have better surface quality, improved added value of the parts, and have better environmental protection performance, higher fire resistance and higher corrosion resistance. In addition, the weight of zinc-coated parts of the same thickness is greatly reduced, thereby improving the use efficiency of the parts.
[0020] (2) The present invention uses component B and component C to work synergistically, which can not only activate the zinc-aluminum-magnesium powder and improve the adhesion of the zinc-aluminum-magnesium powder, but also promote the reaction of the zinc-aluminum-magnesium powder with the steel matrix, thereby promoting the formation of the zinc-aluminum-magnesium coating and enhancing the bonding strength between the zinc-aluminum-magnesium coating and the matrix. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is an appearance diagram of a gasket with a zinc-aluminum-magnesium coating prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0022] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0023] Example 1
[0024] A method for preparing a spray material for spray-depositing a zinc-aluminum-magnesium coating comprises the following steps:
[0025] (1) 12.3 g of silver nitrate and 9.8 g of nickel sulfamate were placed in 100 ml of water and stirred. During the stirring process, 7.5 g of titanium dioxide and 5.6 g of TX-10 were added until the mixture was uniformly stirred to obtain component B;
[0026] (2) 28.4 g of stannous sulfate was added to 100 ml of water and stirred. During the stirring process, 10.4 g of sodium hypophosphite and 3.8 g of sodium molybdate were added. Finally, 2.5 g of sodium hydroxide and 1.9 g of ammonia water were added until the mixture was uniformly stirred to obtain component C.
[0027] (3) Component B with a mass percentage of 45% and component C with a mass percentage of 55% are stirred evenly. After reacting for 90 seconds, component A (15g zinc aluminum magnesium powder, 2kg zirconium beads and 1kg steel balls) with a mass ratio of component A to the total amount of component B and component C being 201:10 are added and mixed evenly to obtain a spray material for spray-deposited zinc aluminum magnesium coating.
[0028] The spray material of the spray-deposited zinc-aluminum-magnesium coating is subjected to a spray-deposited coating preparation process to form a zinc-aluminum-magnesium coating, comprising:
[0029] S1: Add the spray material of the spray-deposited zinc-aluminum-magnesium coating into the spray material chamber of the spray deposition plating device; then pickle 1kg of standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash the gasket with alkali to remove the oil stain, and then add it into the spray deposition chamber from the feed inlet.
[0030] S2: After the nozzle is turned on to perform spray deposition plating on the rotating gasket for 480 seconds, a dense and uniform zinc-aluminum-magnesium coating is formed on the surface of the gasket.
[0031] Example 2
[0032] A method for preparing a spray material for spray-depositing a zinc-aluminum-magnesium coating comprises the following steps:
[0033] (1) 13.2 g of silver nitrate and 10.8 g of nickel sulfamate were placed in 100 ml of water and stirred. During the stirring process, 8.4 g of titanium dioxide and 6.6 g of TX-10 were added until the mixture was uniformly stirred to obtain component B;
[0034] (2) 30.2 g of stannous sulfate was added to 100 ml of water and stirred. During the stirring process, 10.8 g of sodium hypophosphite and 3.3 g of sodium molybdate were added. Finally, 2.2 g of aluminum hydroxide, 1.5 g of copper hydroxide and 1.2 g of ammonia water were added until the mixture was uniformly stirred to obtain component C.
[0035] (3) 40% by mass of component B and 60% by mass of component C are stirred evenly, and after reacting for 90 seconds, component A (20g zinc aluminum magnesium powder, 2kg zirconium beads and 2kg alumina beads) with a mass ratio of component A to the total amount of component B and component C being 201:14 is added and mixed evenly to obtain a spray material for spray-deposited zinc aluminum magnesium coating.
[0036] The spray material of the spray-deposited zinc-aluminum-magnesium coating is subjected to a spray-deposited coating preparation process to form a zinc-aluminum-magnesium coating, comprising:
[0037] S1: Add the spray material of the spray-deposited zinc-aluminum-magnesium coating into the spray material chamber of the spray deposition plating device; then pickle 1kg of standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash the gasket with alkali to remove the oil stain, and then add it into the spray deposition chamber from the feed inlet.
[0038] S2: After opening the nozzle to perform spray deposition plating on the rotating gasket for 720 seconds, a dense and uniform zinc-aluminum-magnesium coating is formed on the surface of the gasket.
[0039] Example 3
[0040] A method for preparing a spray material for spray-depositing a zinc-aluminum-magnesium coating comprises the following steps:
[0041] (1) 14 g of silver nitrate and 11.6 g of nickel sulfamate were placed in 100 ml of water and stirred. During the stirring process, 8.4 g of titanium dioxide and 6.9 g of TX-10 were added until the mixture was uniformly stirred to obtain component B;
[0042] (2) 31 g of stannous sulfate was added to 100 ml of water and stirred. During the stirring process, 11.4 g of sodium hypophosphite and 4.2 g of sodium molybdate were added. Finally, 3.1 g of sodium hydroxide, 1 g of ferrous hydroxide, 0.8 g of copper hydroxide and 0.5 g of ammonia water were added until the mixture was uniformly stirred to obtain component C.
[0043] (3) 50% by mass of component B and 50% by mass of component C are stirred evenly, and after reacting for 90 seconds, component A (30g of zinc-aluminum-magnesium powder, 2.5kg of steel balls and 2.5kg of alumina balls) with a mass ratio of component A to the total amount of component B and component C being 201:12 is added and mixed evenly to obtain a spray material for spray-deposited zinc-aluminum-magnesium coating.
[0044] The spray material of the spray-deposited zinc-aluminum-magnesium coating is subjected to a spray-deposited coating preparation process to form a zinc-aluminum-magnesium coating, comprising:
[0045] S1: Add the spray material of the spray-deposited zinc-aluminum-magnesium coating into the spray material chamber of the spray deposition plating device; then pickle 1kg of standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash the gasket with alkali to remove the oil stain, and then add it into the spray deposition chamber from the feed inlet.
[0046] S2: After the nozzle is turned on to perform spray deposition plating on the rotating gasket for 960 seconds, a dense and uniform zinc-aluminum-magnesium coating is formed on the surface of the gasket.
[0047] Comparative Example 1
[0048] A spray deposition coating preparation process forms a zinc-aluminum-magnesium coating, comprising:
[0049] (1) The workpiece to be plated is a standard gasket with an outer diameter of Φ30 mm, an inner diameter of Φ20 mm, and a thickness of 2 mm. The surface area of the workpiece to be plated is approximately 0.12 m 2 .
[0050] (2) Add 15g of zinc-aluminum-magnesium powder to 1000ml of water, then add 2kg of zirconium beads and 1kg of steel beads, mix well, and add to the spray material chamber of the spray deposition plating device; then pickle 1kg of standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash with alkaline to remove the oil stains on the gasket, and then add it to the spray deposition chamber from the feed inlet.
[0051] (3) After the nozzle was opened to perform spray deposition plating on the rotating gasket for 480 seconds, no zinc-aluminum-magnesium plating layer was formed on the surface of the gasket.
[0052] Comparative Example 2
[0053] A method for preparing a spray material for spray-deposited galvanized coating comprises the following steps:
[0054] (1) 12.3 g of silver nitrate and 9.8 g of nickel sulfamate were placed in 100 ml of water and stirred. During the stirring process, 7.5 g of titanium dioxide and 5.6 g of TX-10 were added until the mixture was uniformly stirred to obtain component B;
[0055] (2) 28.4 g of stannous sulfate was added to 100 ml of water and stirred. During the stirring process, 10.4 g of sodium hypophosphite and 3.8 g of sodium molybdate were added. Finally, 2.5 g of sodium hydroxide and 1.9 g of ammonia water were added until the mixture was uniformly stirred to obtain component C.
[0056] (3) Component B with a mass percentage of 45% and component C with a mass percentage of 55% are stirred evenly. After reacting for 90 seconds, component A (15g zinc powder, 2kg zirconium beads and 1kg steel balls) with a mass ratio of 20:1 between component A and the total amount of component B and component C are added and mixed evenly to obtain a spray material for spray-deposited galvanized coating.
[0057] The spray material of the spray-deposited zinc coating is subjected to a spray-deposited zinc coating preparation process to form a zinc coating, comprising:
[0058] S1: Add the spray material of the spray-deposited galvanized coating obtained above into the spray material chamber; then pickle 1kg of standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash the gasket with alkali to remove the oil stain, and then add it into the spray deposition chamber from the feed inlet.
[0059] S2: After the nozzle is turned on to perform spray deposition plating on the rotating gasket for 480 seconds, no zinc plating layer is formed on the surface of the gasket.
[0060] The deposition aid for the spray-deposited zinc-aluminum-magnesium coating of the present invention cannot activate the zinc powder, so zinc plating cannot be formed on the surface of the substrate.
[0061] Effect example
[0062] The coating density, coating bonding strength, coating average thickness, and corrosion resistance of the spray-deposited zinc-aluminum-magnesium coating gaskets of Examples 1 to 3 were tested, and the results are shown in Table 1 below.
[0063] The density of the coating is determined by measuring the porosity.
[0064] Plating bonding strength test: Use the scribing and cross-grid method, refer to GC / T 5270-2005, and observe whether there is any lifting or shedding of the coating at the cross-intersection position of the scribing.
[0065] Neutral salt spray test: The sample is suspended in a salt spray chamber and sprayed continuously. The test environment temperature is 25°C and the corrosion resistance process is in NaCl salt spray with a mass fraction of 5%.
[0066] Table 1
[0067]
[0068] The silver nitrate, titanium dioxide, nickel sulfamate, TX-10, sodium hypophosphite, stannous sulfate, sodium molybdate, sodium hydroxide and weak base of the present invention synergistically improve the electrochemical activation, hydrothermal activation and interfacial activation of zinc-aluminum-magnesium powder, and improve the bonding force between the deposited layer and the substrate. If one of the substances is missing, the spray material for spray-depositing the zinc-aluminum-magnesium coating cannot form a zinc-aluminum-magnesium coating on the surface of the substrate. Even if the zinc-aluminum-magnesium coating is formed, its bonding force with the substrate is weak, and it falls off, and the corrosion resistance decreases: for example, if silver nitrate is missing, the zinc-aluminum-magnesium coating cannot be generated. If sodium hypophosphite or stannous sulfate is missing, the hydrothermal activation effect is reduced, and the density and uniformity of the generated zinc-aluminum-magnesium coating are poor, and it is very easy to fall off, and the corrosion resistance is poor. If titanium dioxide and TX-10 are missing, the generated zinc-aluminum-magnesium coating is very easy to fall off. If nickel sulfamate or sodium molybdate is missing, the wear resistance of the zinc-aluminum-magnesium coating is significantly reduced. If sodium hydroxide or weak base is missing, the zinc-aluminum-magnesium coating cannot be formed on the surface of the substrate.
[0069] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A deposition aid for spray-deposited zinc-aluminum-magnesium coatings, It is characterized in that It includes component B and component C; component B includes silver nitrate, titanium dioxide, nickel sulfamate, TX-10 and water; component C includes sodium hypophosphite, stannous sulfate, sodium molybdate, sodium hydroxide, weak base and water.
2. The deposition aid for spray-deposited zinc-aluminum-magnesium coating as claimed in claim 1, It is characterized in that The mass percentage of component B in the deposition aid is 40% to 50%, and the mass percentage of component C is 50% to 60%.
3. The deposition aid for spray-deposited zinc-aluminum-magnesium coating as claimed in claim 2, It is characterized in that The mass percentage of the B component is 45% to 50%, and the mass percentage of the C component is 50% to 55%.
4. The deposition aid for spray-deposited zinc-aluminum-magnesium coating as claimed in claim 1, It is characterized in that The B component comprises the following components in percentage by mass: 7% to 10% silver nitrate, 4% to 7% titanium dioxide, 4% to 9% nickel sulfamate, 2% to 5% TX-10 and the balance water.
5. The deposition aid for spray-deposited zinc-aluminum-magnesium coating as claimed in claim 1, It is characterized in that The C component comprises the following components in percentage by mass: 5% to 8% sodium hypophosphite, 8% to 20% stannous sulfate, 1.5% to 3% sodium molybdate, 1% to 2.5% sodium hydroxide, 1% to 2.5% weak base and the balance water.
6. The deposition aid for spray-deposited zinc-aluminum-magnesium coating as claimed in claim 1, It is characterized in that The weak base is one or more of aluminum hydroxide, copper hydroxide, ferrous hydroxide and ammonia water.
7. A spray material for spray-depositing zinc-aluminum-magnesium coating, It is characterized in that It comprises component A and a deposition aid for spray-deposited zinc-aluminum-magnesium coating according to any one of claims 1 to 6; component A comprises zinc-aluminum-magnesium powder and a spray-deposited medium; and the mass ratio of component A to the deposition aid is 201:(10-20).
8. The spray material for spray-depositing the zinc-aluminum-magnesium coating as claimed in claim 7, It is characterized in that The spray deposition medium is one or two of zirconium beads, alumina beads, and steel beads; the mass ratio of the spray deposition medium to zinc-aluminum-magnesium powder is (165-200):
1.
9. The spray material for spray-depositing the zinc-aluminum-magnesium coating as claimed in claim 1, It is characterized in that The method for preparing the spray material for spray-depositing zinc-aluminum-magnesium coating comprises the following steps: (1) silver nitrate and nickel sulfamate are placed in water and stirred, and titanium dioxide and TX-10 are added during the stirring process until the mixture is stirred evenly to obtain component B; (2) adding stannous sulfate into water and stirring, adding sodium phosphite and sodium molybdate during the stirring process, and finally adding sodium hydroxide and a weak base until the stirring is uniform to obtain component C; (3) Components B and C are stirred evenly, and after reacting for 90 seconds, component A is added to obtain a spray material for spray-deposited zinc-aluminum-magnesium coating.