Multi-component alloy coating as well as preparation method and application thereof

Through ball mill mixing of metal powders such as Ti, Zr, Nb, Co and Cr and laser cladding nitriding technology, a multi-component alloy gradient composite coating was prepared, solving the lack of wear resistance and biocompatibility of existing medical materials. The problem of this paper significantly improves the hardness and corrosion resistance of the material and extends the service life.

CN118957566APending Publication Date: 2024-11-15ZHOUSHAN JIADING PLASTIC MASCH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411030997.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing medical titanium alloys and stainless steel materials are insufficient in the human body, resulting in short service life and high manufacturing cost of precious metal elements. It requires a multi-component alloy material with excellent performance and economical performance. and preparation method.

Method used

The multi-component alloy gradient composite coating is prepared by mixing metal elemental powders such as Ti, Zr, Nb, Co and Cr through ball milling, combined with laser cladding and laser nitriding technology, to improve the hardness and wear resistance of the material surface, and through adjustment Scanning strategies and nitriding treatment further improve performance.

Benefits of technology

The uniform structure and excellent mechanical properties of the multi-component alloy coating are achieved, the hardness is increased to 750Hv0.1, the corrosion resistance is significantly improved, and the surface hardness after nitriding reaches 1225Hv0.1, extending the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957566A_ABST
    Figure CN118957566A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of alloy coating preparation, in particular to a multi-component alloy coating and a preparation method and application thereof. The invention provides a preparation method of a multi-component alloy coating, which comprises the following steps: ball-milling and mixing metal elementary substance powder, mixing with a binder, coating on the surface of a matrix alloy, and then carrying out laser cladding to obtain a reinforced coating, and under the atmosphere of protective gas, laser scanning is conducted on the strengthened coating, finally, the surface of the coating is ground and polished, and the multi-component alloy coating is obtained. Wherein the metal elementary substance powder is metal elementary substance powder of Ti, Zr, Nb, Co and Cr. The HEAs surface is golden yellow, the highest hardness is improved to 1225Hv < 0.1 >, and the depth of a nitriding layer is three times that of a base body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy coating preparation, and in particular to a multi-component alloy coating and a preparation method and application thereof. Background Art

[0002] Biomedical materials are new materials that are specially used to detect, treat, repair and replace human tissues and organs and improve their functions, usually including metals, ceramics and polymers. Medical metal materials are widely used due to their excellent mechanical properties and stability, but for implantation in the human body, there are more stringent requirements for the material itself. Not only must its elastic modulus match that of human bones and its mechanical properties meet the requirements of long-term use, but it must also have good biocompatibility with the human body and not produce biological toxicity to the human body, in order to ensure personal safety and avoid secondary injuries.

[0003] Currently, commonly used medical titanium alloys and stainless steel materials often cannot exist in the human body for a long time due to their poor wear resistance, corrosion resistance and biological properties. In response to this, some multi-component alloys (HEAs) with medical potential have emerged. In order to meet various strict requirements, one or more precious metal elements are generally used, and their manufacturing costs are too expensive. Therefore, a high-performance and economical alloy material and a more economical and efficient preparation method are needed. Therefore, laser cladding technology is to prepare HEAs coatings on the surface of materials, which can not only greatly reduce manufacturing costs, but also make the substrate have the superior performance of large HEAs.

[0004] Based on this, in view of the shortcomings in the prior art, the present invention proposes a new HEAs powder and preparation method and a HEAs coating preparation method, which is an alloy formed by five or more metals and each alloy content is between 5% and 35%, and has extremely low biological toxicity to the human body. It is deposited on the substrate by laser cladding technology, effectively improving the hardness and wear and corrosion resistance of the material surface, and further improving the surface performance and biological activity by laser nitriding treatment. Traditional steel and titanium alloy nitriding will form a thin (1-5μm) and hard and brittle (>2000Hv) nitride layer on the surface of the workpiece, which will damage the fatigue performance and impact resistance to a certain extent. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a laser nitrided multi-element alloy gradient composite coating and its preparation method and application. The present invention prepares a new multi-element alloy coating through laser cladding to improve the low surface hardness and poor wear resistance of titanium alloy implants; through laser nitriding technology, a gradient composite coating is prepared to further improve its surface hardness and increase the service life of the titanium alloy.

[0006] In a first aspect, the present invention provides a method for preparing a multi-component alloy coating in an optional embodiment, comprising the following steps:

[0007] S1: After ball milling, the metal powder is mixed with a binder and coated on the surface of the base alloy, and then laser cladding is performed to obtain a strengthening coating;

[0008] S2: In an atmosphere of protective gas, laser scanning the strengthening coating, and finally grinding and polishing the surface of the coating to obtain a multi-component alloy coating;

[0009] Wherein, the metal single substance powder is metal single substance powder of Ti, Zr, Nb, Co and Cr.

[0010] In the present invention, the number of the strengthening coating layers may be 1-3 layers.

[0011] Preferably, in the metal element powder, the molar ratio of Ti, Zr, Nb, Co and Cr is (5-35): (5-35): (5-35): (5-35): (5-35).

[0012] Furthermore, in the metal element powder, the molar ratio of Ti, Zr, Nb, Co and Cr is 20:20:20:20:20.

[0013] Preferably, in step S2, the power of the laser scanning is 250-300 W, preferably 300 W; and / or, the speed of the laser scanning is 900-1000 mm / s, preferably 950 mm / s. The spacing of the laser scanning is 0.03-0.05 mm, preferably 0.04 mm; and / or, the number of laser scanning is 8-12 times, preferably 10 times.

[0014] Preferably, in step S1, the power of the laser cladding is 2.5-3.5KW, preferably 3KW; and / or, the rate of the laser cladding is 6-10mm / s, preferably 8mm / s. The rotation speed of the ball mill is 100-140r / min, preferably 120r / min, and the time is 1.5-2.5h, preferably 2h; and / or, during the ball milling, the mass ratio of the grinding balls to the powder is 1:6-8, preferably 1:7.

[0015] Preferably, the matrix alloy is selected from one of titanium alloy TC4 material, 316 stainless steel, nickel-based alloy or 38 chromium-molybdenum-aluminum high-grade nitrided steel; and / or the binder is anhydrous alcohol; and / or the protective gas is nitrogen or a mixture of nitrogen and argon.

[0016] Before coating the metal element powder, the surface to be deposited on the base alloy is ground, cleaned and dried.

[0017] In a second aspect, the present invention provides, in an optional embodiment, a multi-component alloy coating prepared by the above-mentioned preparation method.

[0018] In a third aspect, the present invention provides, in an optional embodiment, a multi-component alloy coating prepared by the above-mentioned preparation method and the application of the multi-component alloy coating in biomedical materials.

[0019] Compared with the prior art, the present invention has one of the following beneficial effects:

[0020] 1. The present invention proposes an alloy powder of Ti-Zr-Nb-Cr-Co components, deposits a new HEAs coating on the surface of a TC4 alloy to enhance the surface properties of the TC4 alloy, uses a fiber laser to prepare the coating, changes the coating preparation strategy by an adjustable spot size, thereby obtaining HEAs coatings with different properties, and affects the dilution rate by changing the scanning rate, overlap rate, and number of stacking layers, thereby controlling the microstructure and properties of the HEAs coating.

[0021] 2. The coating has a uniform organizational structure and good formability, excellent mechanical properties and corrosion resistance. Its hardness is up to 750Hv0.1, which is twice that of the substrate, and has the lowest corrosion current density. Then, laser gas nitridation is further proposed to regulate the organization and surface modification of HEAs coatings to further improve its surface properties. The surface of HEAs after nitridation is golden yellow, the maximum hardness is increased to 1225Hv0.1, and the depth of the nitriding layer is three times that of the substrate.

[0022] 3. The reinforcing phase nitride in the composite coating formed after laser nitriding presents a gradient distribution with dense surface and loose interior. This not only further improves the hardness and wear resistance of the multi-element coating, but also ensures the overall toughness of the coating and effectively prevents the coating from cracking. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 This is a morphology diagram of the alloy powder after ball milling in Example 1 of the present invention;

[0025] Figure 2 This is a sample diagram of a multi-component alloy coating prepared in Comparative Example 1 of the present invention;

[0026] Figure 3XRD patterns of the multi-component alloy coatings prepared in Comparative Examples 1-3 of the present invention;

[0027] Figure 4 This is a SEM test result diagram of the multi-component alloy coating prepared in Comparative Examples 1-3 of the present invention;

[0028] Figure 5 The performance result curves of the multi-component alloys prepared in Comparative Examples 1-3 of the present invention, wherein a is a hardness curve and b is a polarization curve;

[0029] Figure 6 This is a surface morphology image of the multi-component alloy coating prepared in Example 1 of the present invention;

[0030] Figure 7 It is a hardness curve diagram of the multi-component alloy coating prepared in Example 1 of the present invention and the alloy coating prepared in Comparative Example 4;

[0031] Figure 8 This is a SEM test result diagram of the multi-component alloy coating prepared in Example 1 of the present invention;

[0032] Fig. 9 This is a SEM test result diagram of the alloy coating prepared in Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0034] The following is a specific example to illustrate the solution of the present invention.

[0035] Example 1

[0036] This embodiment provides a method for preparing a multi-component alloy coating, comprising the following steps:

[0037] 1. Prepare TiZrNbCoCr multi-component alloy powder, mix the powder according to the molar ratio: Ti = 20%, Zr = 20%, Nb = 20%, Co = 20%, Cr = 20%, use a high-precision electronic balance to weigh each metal powder, and the total atomic percentage is 100%;

[0038] 2. The mixed metal powders were ball milled, the protective atmosphere was argon, the mass ratio of grinding balls to mixed powders was 1:7, the rotation speed was 120r / min, the ball milling time was 2h, the powders were taken out and placed in a vacuum drying furnace for drying, and then placed in a drying dish for later use. The results are as follows: Figure 1 ;

[0039] 3. The coating deposition substrate pretreatment process is as follows: the surface of the substrate TC4 alloy (Ti-6Al-4V) to be deposited is polished, cleaned and dried by a metallographic polishing machine for standby use;

[0040] 4. The powder obtained in step 2 is mixed with anhydrous alcohol to form a slurry, and spread on the substrate prepared in step 3. The thickness of the powder bed is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with the powder is placed in an atmosphere protection box, and pure argon gas is introduced for washing before laser scanning;

[0041] 5. Use a continuous wave output semiconductor laser to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning. The laser process parameters are: laser power of 3kW, scanning speed of 8mm / s, overlap rate of 65%. After the laser scanning is completed, pure argon gas is continuously introduced until the sample is cooled to prevent oxidation during the cooling process, and a layer of strengthening coating is obtained;

[0042] 6. After grinding the surface of a layer of strengthening coating to remove oxidized impurities, the slurry in step 4 is spread evenly on the surface of a layer of strengthening coating. The thickness of the powder bed is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with powder is placed in an atmosphere protection box. Pure argon gas is introduced for purge before laser scanning. A continuous wave output semiconductor laser is used to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning. The laser process parameters are as follows: laser power is 3kW, scanning speed is 8mm / s, overlap rate is 65%. After the laser scanning is completed, pure argon gas is continuously introduced until the sample is cooled to prevent oxidation during the cooling process, and a second layer of strengthening coating is obtained.

[0043] 7. After the surface of the second layer of strengthening coating is polished to remove oxidized impurities, the slurry in step 4 is spread evenly on the surface of the second layer of strengthening coating. The thickness of the powder bed is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with powder is placed in an atmosphere protection box. Pure argon gas is introduced for purge before laser scanning. A continuous wave output semiconductor laser is used to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning. The laser process parameters are as follows: laser power is 3kW, scanning speed is 8mm / s, overlap rate is 65%. After the laser scanning is completed, pure argon gas is continuously introduced until the sample is cooled to prevent oxidation during the cooling process, and a three-layer strengthening coating is obtained.

[0044] 8. Place the three-layer strengthening coating in an atmosphere protection box filled with a 1:1 mixture of pure nitrogen and argon, and wash the gas;

[0045] 9. Use a pulse wave galvanometer fiber laser to scan the H3 multi-component alloy coating prepared in step 6, using a bow-shaped scanning method, wherein the laser process parameters are: laser power of 300 W, scanning speed of 950 mm / s, scanning spacing of 0.04 mm, scanning times of 10 times, and nitrogen / argon mixed gas is continuously introduced during the period until the sample cools down;

[0046] 10. The newly obtained TiZrNbCrCo multi-component alloy coating cross section was polished to a mirror surface to obtain a multi-component alloy coating, which was recorded as HEA-N. Figure 6 .

[0047] Example 2

[0048] This embodiment provides a method for preparing a multi-component alloy coating, comprising the following steps: The difference between this embodiment and Example 1 is that the base alloy in step 3 is 316 stainless steel, and the remaining steps are the same as those in Example 1.

[0049] Example 3

[0050] This embodiment provides a method for preparing a multi-component alloy coating, comprising the following steps: The difference between this embodiment and Example 1 is that the base alloy in step 3 is 38 chromium-molybdenum-aluminum high-grade nitrided steel, and the remaining steps are the same as those in Example 1.

[0051] Comparative Example 1

[0052] This comparative example provides a method for preparing a multi-component alloy coating, comprising the following steps:

[0053] 1. Prepare TiZrNbCoCr multi-component alloy powder, mix the powder according to the molar ratio: Ti = 20%, Zr = 20%, Nb = 20%, Co = 20%, Cr = 20%, use a high-precision electronic balance to weigh each metal powder, and the total atomic percentage is 100%;.

[0054] 2. The mixed metal powders were ball milled, the protective atmosphere was argon, the mass ratio of grinding balls to mixed powders was 1:7, the rotation speed was 120r / min, the ball milling time was 2h, the powders were taken out and placed in a vacuum drying furnace for drying, and then placed in a drying dish for later use. The results are as follows: Figure 1 ;

[0055] 3. The coating deposition substrate pretreatment process is as follows: the surface of the substrate TC4 alloy (Ti-6Al-4V) to be deposited is polished, cleaned and dried by a metallographic polishing machine for standby use;

[0056] 4. The powder obtained in step 2 is mixed with anhydrous alcohol to form a slurry, and spread on the substrate prepared in step 3. The thickness of the powder bed is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with the powder is placed in an atmosphere protection box, and pure argon gas is introduced for washing before laser scanning;

[0057] 5. Use a continuous wave output semiconductor laser to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning. The laser process parameters are: laser power of 3kW, scanning speed of 8mm / s, overlap rate of 65%. After the laser scanning is completed, pure argon gas is continuously introduced until the sample is cooled to prevent oxidation during the cooling process, and a layer of strengthening coating is obtained;

[0058] 6. The outermost layer of the obtained strengthening coating is ground and polished to a mirror surface using a metallographic grinder and polisher to obtain a multi-component alloy coating, which is recorded as H1.

[0059] Characterize and test H1: XRD test results are as follows Figure 3 As shown in the H1 curve, the figure proves that the obtained coating is a multi-component alloy coating, and the coating is a single BCC phase solid solution; the coating structure morphology is observed using SEM, such as Figure 4 As shown in H1, the H1 coating structure is composed of dendrites and inter-dendritic spaces, and is evenly distributed. The microhardness of the H1 multi-component alloy coating was measured using a digital Vickers microhardness tester. The results are shown in Figure 5 As shown in the H1 curve in a, the average hardness of the H1 multi-component alloy coating reaches 581.4Hv0.1, which is 1.81 times higher than the substrate hardness (320Hv0.1); the electrochemical performance test is carried out in 3.5% NaCl solution, as shown in Figure 5 As shown in the H1 curve of b, the corrosion potential of the H1 coating is -0.313 V, and the corrosion current density is 9.282×10 -6 A.cm -2 , which has corrosion resistance comparable to that of the substrate and has a lower corrosion rate than the substrate.

[0060] Comparative Example 2

[0061] This comparative example provides a method for preparing a multi-component alloy coating, comprising the following steps:

[0062] 1. Prepare TiZrNbCoCr multi-component alloy powder, mix the powder according to the molar ratio: Ti = 20%, Zr = 20%, Nb = 20%, Co = 20%, Cr = 20%, use a high-precision electronic balance to weigh each metal powder, and the total atomic percentage is 100%;.

[0063] 2. The mixed metal powders were ball-milled, the protective atmosphere was argon, the mass ratio of grinding balls to mixed powders was 1:7, the rotation speed was 120 r / min, the ball-milling time was 2 h, the powders were taken out and dried in a vacuum drying furnace, and then stored in a drying dish for later use;

[0064] 3. The coating deposition substrate pretreatment process is as follows: the surface of the substrate TC4 alloy (Ti-6Al-4V) to be deposited is polished, cleaned and dried by a metallographic polishing machine for standby use;

[0065] 4. The powder obtained in step 2 is mixed with anhydrous alcohol to form a slurry, and spread on the substrate prepared in step 3. The thickness of the powder bed is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with the powder is placed in an atmosphere protection box, and pure argon gas is introduced for washing before laser scanning;

[0066] 5. Use a continuous wave output semiconductor laser to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning, and the scanning angle is deflected 180° relative to the H1 multi-component alloy coating. The laser process parameters are: laser power of 3kW, scanning speed of 8mm / s, overlap rate of 65%, and pure argon gas is always continuously introduced during the laser scanning process until the sample cools down to prevent oxidation during the cooling process;

[0067] 6. After grinding the surface of a layer of strengthening coating to remove oxidized impurities, the slurry in step 4 is spread evenly on the surface of a layer of strengthening coating. The thickness of the powder bed is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with powder is placed in an atmosphere protection box. Pure argon gas is introduced for purge before laser scanning. A continuous wave output semiconductor laser is used to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning, and the scanning angle is deflected by 180° relative to the H1 multi-component alloy coating. The laser process parameters are as follows: laser power is 3kW, scanning speed is 8mm / s, overlap rate is 65%, and pure argon gas is continuously introduced during the laser scanning process until the sample is cooled to prevent oxidation during the cooling process, thereby obtaining a second layer of strengthening coating.

[0068] 7. The outermost layer of the obtained two-layer strengthening coating is ground and polished to a mirror surface using a metallographic grinder and polisher to obtain a multi-component alloy coating, which is recorded as H2.

[0069] Characterize and test H2: XRD test results are as follows Figure 3 As shown in the H2 curve, the figure proves that the obtained coating is a multi-component alloy coating. From the figure, it can be seen that compared with the single BCC solid solution phase in H1, a small amount of intermetallic compounds (Laves phase) appear in the H2 coating; the coating morphology is observed using SEM, as shown in Figure 4As shown in Figure 1, the H2 coating structure consists of dendrites and interdendritic spaces, and is evenly distributed. The structure of the H2 coating is significantly refined, and fine lamellar structures are observed between the dendrites. The microhardness of the H2 multi-component alloy coating was measured using a digital Vickers microhardness tester. The results are shown in Figure 1. Figure 5 As shown in the H2 curve in a, the average hardness of the H2 multi-component alloy coating reaches 595.4Hv0.1, which is 1.9 times higher than the substrate hardness (320Hv0.1); the electrochemical performance test is carried out in 3.5% NaCl solution, as shown in Figure 5 As shown in the H2 curve in b, compared with the H1 multi-component alloy coating, the corrosion potential of the H2 coating is increased to -0.286 V, and the corrosion current density is reduced to 6.460×10 -6 A.cm -2 , showing better corrosion resistance than the substrate and H1 coating.

[0070] Comparative Example 3

[0071] This comparative example provides a method for preparing a multi-component alloy coating, comprising the following steps:

[0072] 1. Prepare TiZrNbCoCr multi-component alloy powder, mix the powder according to the molar ratio: Ti = 20%, Zr = 20%, Nb = 20%, Co = 20%, Cr = 20%, use a high-precision electronic balance to weigh each metal powder, and the total atomic percentage is 100%;

[0073] 2. The mixed metal powders were ball-milled, the protective atmosphere was argon, the mass ratio of grinding balls to mixed powders was 1:7, the rotation speed was 120 r / min, the ball-milling time was 2 h, the powders were taken out and dried in a vacuum drying furnace, and then stored in a drying dish for later use;

[0074] 3. The coating deposition substrate pretreatment process is as follows: the surface of the substrate TC4 alloy (Ti-6Al-4V) to be deposited is polished, cleaned and dried by a metallographic polishing machine for standby use;

[0075] 4. The powder obtained in step 2 is mixed with anhydrous alcohol to form a slurry, and spread on the substrate prepared in step 3. The thickness of the powder bed is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with the powder is placed in an atmosphere protection box, and pure argon gas is introduced for washing before laser scanning;

[0076] 5. Use a continuous wave output semiconductor laser to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning, and the scanning angle is deflected 180° relative to the H2 multi-component alloy coating. The laser process parameters are: laser power of 3kW, scanning speed of 8mm / s, overlap rate of 65%, and pure argon gas is always continuously introduced during the laser scanning process until the sample cools down to prevent oxidation during the cooling process;

[0077] 6. After grinding the surface of a layer of strengthening coating to remove oxidized impurities, the slurry in step 4 is spread evenly on the surface of a layer of strengthening coating. The thickness of the powder bed is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with powder is placed in an atmosphere protection box. Pure argon gas is introduced for purge before laser scanning. A continuous wave output semiconductor laser is used to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning, and the scanning angle is deflected by 180° relative to the H2 multi-component alloy coating. The laser process parameters are as follows: laser power is 3kW, scanning speed is 8mm / s, overlap rate is 65%, and pure argon gas is always continuously introduced during the laser scanning process until the sample is cooled to prevent oxidation during the cooling process, thereby obtaining a second layer of strengthening coating.

[0078] 7. After the surface of the second-layer strengthening coating is polished to remove oxidized impurities, the slurry in step 4 is spread evenly on the surface of the second-layer strengthening coating. The powder bed thickness is 1.0±0.2mm. In order to prevent the alloy from oxidizing during the melting process, the substrate with the powder is placed in an atmosphere protection box. Pure argon gas is introduced for purge before laser scanning. A continuous wave output semiconductor laser is used to perform laser scanning on the preset multi-component alloy powder bed. The scanning adopts a straight-line scanning, and the scanning angle is deflected by 180° relative to the H2 multi-component alloy coating. The laser process parameters are as follows: laser power is 3kW, scanning speed is 8mm / s, overlap rate is 65%, and pure argon gas is continuously introduced during the laser scanning process until the sample is cooled to prevent oxidation during the cooling process, thereby obtaining a three-layer strengthening coating.

[0079] 8. The outermost layer of the three-layer strengthening coating was ground and polished to a mirror surface using a metallographic grinder and polisher to obtain a multi-component alloy coating, which was recorded as H3.

[0080] Characterize and test H3: XRD test results are as follows Figure 3 As shown in the H3 curve, the figure proves that the obtained coating is a multi-component alloy coating. From the figure, it can be seen that the BCC peak position of the H3 coating is further shifted compared with the H2, and a small amount of α-Ti phase is detected; the coating structure morphology is observed using SEM, as shown Figure 4As shown in the figure, the H3 coating structure is composed of dendrites and interdendritic spaces. Compared with the H2 multi-component alloy coating, the H3 coating structure is equiaxed crystals with uniform distribution. The microhardness of the H3 multi-component alloy coating was measured using a digital Vickers microhardness tester. The results are shown in Figure 5 As shown in the H3 curve in a, the average hardness of the H3 multi-component alloy coating reaches 747.7Hv0.1, which is 2.34 times higher than the substrate hardness (320Hv0.1), and the hardness is further improved compared with the H1 and H2 multi-component alloy coatings. This also shows that the multi-component alloy coating with three deposition times effectively improves its mechanical properties; the electrochemical performance test was carried out in 3.5% NaCl solution, as shown in Figure 5 As shown in the H3 curve of b, the corrosion potential of the H3 coating is -0.286 V, and the corrosion current density is 1.986×10 -5 A.cm -2 , compared with the H2 multi-component alloy coating, it has a certain decrease.

[0081] Comparative Example 4

[0082] This comparative example provides a method for preparing an alloy coating, comprising the following steps:

[0083] 1. Grind the base TC4 alloy (Ti-6Al-4V) to remove oxidized impurities, polish and ultrasonically clean it, then blow dry it and set it aside;

[0084] 2. Place the matrix TC4 alloy obtained in step 1 into an atmosphere protection box filled with a 1:1 mixture of pure nitrogen and argon, and wash the gas;

[0085] 3. Use a pulse wave galvanometer fiber laser to scan the H3 multi-component alloy coating prepared in step 6, using a bow-shaped scanning method, where the laser process parameters are: laser power of 300 W, scanning speed of 950 mm / s, scanning spacing of 0.04 mm, scanning times of 10 times, during which nitrogen / argon mixed gas is continuously introduced until the sample is cooled; an alloy coating is obtained, which is recorded as TC4-N.

[0086] Experimental example

[0087] The microhardness of HEA-N multi-component alloy coating and TC4-N alloy coating was measured. Figure 7 As shown in the curve in, the maximum hardness of the HEA-N multi-component alloy coating reaches 1250Hv0.1, which is 3.91 times higher than the substrate hardness (320Hv0.1), and the hardness is greatly improved compared with the H1, H2 and H3 multi-component alloy coatings; the microstructure of the HEA-N multi-component alloy coating and the TC4-N alloy coating was observed by SEM, and the results are shown in Figure 8-9 As shown, Figure 8This is the SEM morphology of the HEA-N multi-component alloy coating. Fig. 9 The SEM morphology of the TC4-N alloy coating is shown in Figure 8 In the figure, the diffusely distributed dark particles are nitrides with high nitrogen content. Fig. 9 In the figure, the particles agglomerated on the surface are nitrides, which shows that the reinforcing phase nitrides in the HEA-N multi-component alloy coating present a gradient distribution with dense surface and loose interior. Compared with TC4-N, the HEA-N coating has a deeper nitriding depth of 220μm, which is twice that of the substrate.

[0088] Although the principles of the present invention are described in detail above in conjunction with the preferred embodiments of the present invention, those skilled in the art should understand that the above embodiments are merely explanations of the exemplary implementations of the present invention, and are not intended to limit the scope of the present invention. The details in the embodiments do not constitute limitations on the scope of the present invention, and any obvious changes such as equivalent transformations, simple replacements, etc. based on the technical solution of the present invention, without departing from the spirit and scope of the present invention, fall within the protection scope of the present invention.

Claims

1. A method for preparing a multi-component alloy coating, characterized in that: The following steps are involved: S1: After ball milling, the metal powder is mixed with a binder and coated on the surface of the base alloy, and then laser cladding is performed to obtain a strengthening coating; S2: In an atmosphere of protective gas, laser scanning the strengthening coating, and finally grinding and polishing the surface of the coating to obtain a multi-component alloy coating; Wherein, the metal single substance powder is metal single substance powder of Ti, Zr, Nb, Co and Cr.

2. The method for preparing a multi-component alloy coating according to claim 1, characterized in that: In the metal element powder, the molar ratio of Ti, Zr, Nb, Co and Cr is (5-35): (5-35): (5-35): (5-35): (5-35); and / or, The total molar ratio of the metal element powder is 100%.

3. The method for preparing a multi-component alloy coating according to claim 1, characterized in that: In the metal single substance powder, the molar ratio of Ti, Zr, Nb, Co and Cr is 20:20:20:20:

20.

4. The method for preparing a multi-component alloy coating according to claim 1, characterized in that: In step S2, the power of the laser scanning is 250-350W; and / or, The laser scanning speed is 900-1000 mm / s.

5. The method for preparing a multi-component alloy coating according to claim 1, characterized in that: In step S2, the laser scanning interval is 0.03-0.05 mm; and / or, The laser scanning is performed 8-12 times.

6. The method for preparing a multi-component alloy coating according to claim 1, characterized in that: In step S1, the power of the laser cladding is 2.5-3.5KW; and / or, The laser cladding rate is 6-10 mm / s.

7. The method for preparing a multi-component alloy coating according to claim 1, characterized in that: In step S1, the ball milling speed is 100-140 r / min, and the time is 1.5-2.5 h; and / or, During the ball milling, the mass ratio of the grinding balls to the powder is 1:6-8.

8. The method for preparing a multi-component alloy coating according to claim 1, characterized in that: The matrix alloy is selected from one of titanium alloy TC4 material, 316 stainless steel, nickel-based alloy or 38 chromium-molybdenum-aluminum high-grade nitrided steel; and / or, The binder is anhydrous alcohol; and / or, The protective gas is nitrogen or a mixture of nitrogen and argon.

9. A multi-component alloy coating, characterized in that: The preparation method is described in any one of claims 1 to 8.

10. Use of a multi-component alloy coating prepared by the preparation method according to any one of claims 1 to 8 and the multi-component alloy coating according to claim 9 in biomedical materials.