Corrosion-resistant film for magnesium alloy wheel and preparation method of corrosion-resistant film

By stacking MAO, chemical sealing, PVD high-density inorganic hybridization and high-oxidation-resistant powder coatings on magnesium alloy wheels, the problems of poor corrosion resistance and wear resistance of magnesium alloy wheels are solved, and better corrosion resistance and Adhesion extends the life of the wheel and reduces the risk of combustion.

CN118957703APending Publication Date: 2024-11-15CITIC DICASTAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411139668.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The corrosion resistance and wear resistance of magnesium alloy wheels are poor and flammable, which seriously limits their use on automotive wheels.

Method used

A combined structure of MAO coating, chemical sealing coating, PVD high-density inorganic hybrid coating and high-oxidation powder coating arranged from the inner and outer layer is adopted, including in-situ magnesium oxide composite coating and metal oxide Films and polyester resin-based high-oxidation-resistant powder coatings are used to prepare corrosion-resistant films through microarc oxidation technology, PVD coating and electrostatic spraying processes.

Benefits of technology

The corrosion resistance and wear resistance of magnesium alloy wheels are significantly improved, and by enhancing adhesion and corrosion resistance between the membrane layers, the service life of the wheels is extended and the risk of combustion is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957703A_ABST
    Figure CN118957703A_ABST
Patent Text Reader

Abstract

The invention relates to a corrosion-resistant film for a magnesium alloy wheel and a preparation method of the corrosion-resistant film, and belongs to the technical field of corrosion prevention of magnesium alloy wheels, the corrosion-resistant film for the magnesium alloy wheel comprises a magnesium alloy wheel as a substrate, and an MAO coating, a chemical sealing coating, a PVD high-density inorganic hybrid coating and a high-oxidation-resistance powder coating which are sequentially stacked from inside to outside. On the basis of a micro-arc oxidation technology, zirconium, titanium, ferric salt, nano silicon and macromolecular resin are added into an electrolyte, an MAO coating is generated on the surface of the magnesium alloy wheel in a constant-voltage mode of an adjustable power supply, and then chemical sealing is carried out; a PVD high-density inorganic hybrid coating is obtained through film plating on the chemical sealing coating, physical sealing is carried out, and the adhesive force between film layers and the anti-corrosion capacity are improved; and a high-antioxidant powder coating is sprayed on the PVD high-density inorganic hybrid coating, and protection is performed again, so that the corrosion-resistant and wear-resistant coating of the magnesium alloy wheel, which is good in adhesive force and excellent in corrosion resistance, is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnesium alloy wheel anticorrosion, and in particular to a corrosion-resistant film for magnesium alloy wheels and a preparation method thereof. Background Art

[0002] Magnesium alloy is an alloy composed of other elements added to the magnesium matrix. It has the characteristics of low density, high specific strength and specific stiffness, good damping and shock absorption, strong electromagnetic shielding, excellent machinability, and easy recycling. Its weight is about 2 / 3 of that of magnesium alloy. The application of magnesium alloy wheels has a history of more than 40 years. The research and development and use of magnesium alloy wheels can significantly reduce the weight of the car, reduce energy consumption, and achieve the purpose of energy conservation and environmental protection. However, the corrosion resistance and wear resistance of magnesium metal are poor, and it is flammable, which seriously limits its use in automobile wheels. Therefore, seeking an anti-corrosion coating for magnesium alloy wheels and its preparation method has become one of the technical problems that technicians in this field need to solve urgently.

[0003] Therefore, in view of the problems existing in the prior art, the designers of this case actively studied and improved it, and thus came up with the corrosion-resistant film for magnesium alloy wheels and the preparation method thereof of the present invention. Summary of the invention

[0004] The first purpose of the present invention is to provide a corrosion-resistant film for magnesium alloy wheels in view of the defects of the prior art, such as poor corrosion resistance and wear resistance of metal magnesium and its flammability, which seriously limit its use on automobile wheels.

[0005] The second purpose of the present invention is to provide a method for preparing a corrosion-resistant film for magnesium alloy wheels in view of the defects of the prior art, such as poor corrosion resistance and wear resistance of metallic magnesium and its flammability, which seriously limit its use on automobile wheels.

[0006] To achieve the first object of the present invention, the present invention provides a corrosion-resistant film for a magnesium alloy wheel, the corrosion-resistant film for a magnesium alloy wheel comprising: a magnesium alloy wheel as a substrate, an MAO coating, a chemical sealing coating, a PVD high-density inorganic hybrid coating, and a high-oxidation resistance powder coating stacked from the inside to the outside, wherein: The MAO coating is an in-situ grown magnesium oxide composite coating, the magnesium oxide composite coating further contains nano zirconium, titanium, iron, and polymer resin, and the thickness of the MOA coating is 5-10 μm; The chemical sealing coating is prepared by hybridizing the MAO coating in a chromium-free sealing solution; The PVD high-density inorganic hybrid coating is a metal oxide thin film, the film thickness of the PVD high-density inorganic hybrid coating is 180-220 nm, and the metal oxide thin film contains at least one of niobium, chromium, nickel, titanium, zirconium, and tungsten; The highly anti-oxidation powder coating is prepared by using polyester resin as the resin material, carbon black as the filler, and adding a matting agent. The film thickness of the highly anti-oxidation powder coating is 80-100 μm.

[0007] Optionally, the corrosion-resistant film for magnesium alloy wheels further comprises: a color paint and a high-transparency coating sequentially deposited on the outer surface of the high-oxidation-resistant powder coating.

[0008] To achieve the second object of the present invention, the present invention provides a method for preparing a corrosion-resistant film for a magnesium alloy wheel, the method for preparing a corrosion-resistant film for a magnesium alloy wheel comprising: Execute step S1: Based on the micro-arc oxidation technology, zirconium, titanium, iron salt, nano silicon, and polymer resin are added to the electrolyte, and an MAO coating is generated on the surface of the magnesium alloy wheel under the constant voltage mode of the adjustable power supply, wherein the MAO coating is an in-situ grown magnesium oxide composite coating, and the magnesium oxide composite coating further contains nano zirconium, titanium, iron, and polymer resin; Executing step S2: hybridizing the MAO coating in a chromium-free sealing solution to achieve a chemically sealed coating; Executing step S3: using a PVD process to prepare a PVD high-density inorganic hybrid coating; Execute step S4: generate a high-anti-oxidation powder coating on the outer surface of the PVD high-density inorganic hybrid coating by electrostatic spraying.

[0009] Optionally, the method for preparing the corrosion-resistant film for magnesium alloy wheels further comprises: Execute step S5: adopt an electrostatic spraying process to deposit a color paint and a high-transparency coating on the outer surface of the high-anti-oxidation powder coating in sequence.

[0010] Optionally, in step S1, the voltage of the adjustable power supply in the constant voltage mode is 300 V, the corresponding process time is 7 min, the frequency is 500 Hz, and the duty cycle is 6%.

[0011] Optionally, in step S2, the MAO coating is hybridized in a chromium-free sealing solution to achieve a chemical sealing coating, and the drying temperature of the chemical sealing coating is 120° C. and the drying time is 3 minutes.

[0012] Optionally, in step S3, further comprising: Executing step S31: removing the attached water vapor on the surface and in the micropores of the magnesium alloy wheel by infrared heating; Executing step S32: performing plasma treatment to clean the surface of the magnesium alloy wheel and perform surface modification; Execute step S33: adopt PVD process to prepare PVD high-density inorganic hybrid coating.

[0013] Optionally, the infrared heating uses a heating power of 3.9 kW and a heating time of 30 s; the plasma treatment uses a power of 2 kW and an Ar flow rate of 400 sccm; when the PVD process is used, the background vacuum is 1.0×10 -3 Pa, process vacuum degree is 6.0×10 -1 Pa, the coating power is 10KW, the Ar flow rate is 80sccm, and O as the reaction gas 2 The flow rate is 120 sccm and the sputtering time is 120 s. The metal target material used in the PVD process is at least one of niobium, chromium, nickel, titanium, zirconium and tungsten, and the purity is greater than 99.95%.

[0014] Optionally, in step S4, an electrostatic spraying method is used to generate a high antioxidant powder coating on the outer surface of the PVD high-density inorganic hybrid coating, the electrostatic spraying powder amount is 60g / min, the voltage is 50KV, the static electricity is 50μA, the total gas volume is 5MPa, the baking temperature is 170°C, and the baking time is 15min.

[0015] Optionally, in step S5, the baking temperature of the color paint is 140° C., and the baking time is 20 minutes; the curing temperature of the high-transparency coating is 170° C., and the curing time is 15 minutes. In summary, the method for preparing a corrosion-resistant film for a magnesium alloy wheel of the present invention is based on micro-arc oxidation technology on a magnesium alloy wheel, zirconium, titanium, iron salt, nano-silicon, and polymer resin are added to the electrolyte, and an MAO coating is generated on the surface of the magnesium alloy wheel under a constant voltage mode of an adjustable power supply, followed by chemical sealing; PVD coating is performed on the chemically sealed coating to obtain a PVD high-density inorganic hybrid coating, and physical sealing is performed to improve the adhesion and corrosion resistance between film layers; a high-oxidation resistance powder coating is sprayed on the PVD high-density inorganic hybrid coating, and the MAO coating and the chemically sealed coating are protected again, thereby obtaining a magnesium alloy wheel corrosion-resistant and wear-resistant coating with good adhesion and excellent corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Shown is a schematic diagram of the structure of the corrosion-resistant film for magnesium alloy wheels of the present invention; Figure 2 Shown is a flow chart of the method for preparing a corrosion-resistant film for magnesium alloy wheels according to the present invention. DETAILED DESCRIPTION

[0017] In order to explain the technical content, structural features, objectives and effects of the present invention in detail, the following will be described in detail with reference to embodiments and accompanying drawings.

[0018] See also Figure 1 , Figure 1 The figure shows a schematic diagram of the structure of the corrosion-resistant film for magnesium alloy wheels of the present invention. The corrosion-resistant film for magnesium alloy wheels comprises: a magnesium alloy wheel 10 as a substrate, and a MAO coating 11, a chemical sealing coating 12, a PVD high-density inorganic hybrid coating 13, and a high-oxidation-resistant powder coating 14 are stacked from the inside to the outside in sequence, wherein: The MAO coating 11 is an in-situ grown magnesium oxide composite coating, the magnesium oxide composite coating further contains nano zirconium, titanium, iron, and polymer resin, and the thickness of the MAO coating 11 is 5-10 μm; The chemical sealing coating 12 is prepared by hybridizing the MAO coating 11 in a chromium-free sealing solution; The PVD high-density inorganic hybrid coating 13 is a metal oxide thin film, the film thickness of the PVD high-density inorganic hybrid coating 13 is 180-220 nm, and the metal oxide thin film contains at least one of niobium, chromium, nickel, titanium, zirconium, and tungsten; The highly anti-oxidation powder coating 14 is prepared by using polyester resin as the resin material, carbon black as the filler, and adding a matting agent. The film thickness of the highly anti-oxidation powder coating 14 is 80-100 μm.

[0019] Preferably, the corrosion-resistant film for magnesium alloy wheels further comprises: a color paint 15 and a high-transparency coating 16 sequentially deposited on the outer surface of the high-oxidation-resistant powder coating 14 .

[0020] See also Figure 2 , and refer to Figure 1 , Figure 2 The flowchart of the method for preparing the corrosion-resistant film for magnesium alloy wheels of the present invention is shown. The method for preparing the corrosion-resistant film for magnesium alloy wheels comprises: Execute step S1: Based on the micro-arc oxidation technology, zirconium, titanium, iron salt, nano silicon, and polymer resin are added to the electrolyte, and an MAO coating 11 is generated on the surface of the magnesium alloy wheel 10 in a constant voltage mode of an adjustable power supply. The MAO coating 11 is an in-situ grown magnesium oxide composite coating, and the magnesium oxide composite coating further contains nano zirconium, titanium, iron, and polymer resin; Executing step S2: hybridizing the MAO coating 11 in a chromium-free sealing solution to achieve a chemical sealing coating 12; Execute step S3: adopt PVD process to prepare PVD high-density inorganic hybrid coating 13 to further achieve physical sealing; Execute step S4: generate a high-anti-oxidation powder coating 14 on the outer surface of the PVD high-density inorganic hybrid coating 13 by electrostatic spraying.

[0021] Preferably, the method for preparing the corrosion-resistant film for magnesium alloy wheels further comprises: Execute step S5: adopt an electrostatic spraying process to deposit a color paint 15 and a high-transparency coating 16 on the outer surface of the high-anti-oxidation powder coating 14 in sequence.

[0022] As a specific implementation, in step S1, the voltage of the adjustable power supply in the constant voltage mode is 300 V, the corresponding process time is 7 minutes, the frequency is 500 Hz, and the duty cycle is 6%.

[0023] In step S2, the MAO coating 11 is hybridized in a chromium-free sealing solution to achieve a chemical sealing coating 12. The drying temperature of the chemical sealing coating 12 is 120°C and the drying time is 3 minutes.

[0024] In step S3, further comprising: Executing step S31: removing the attached water vapor on the surface and in the micropores of the magnesium alloy wheel by infrared heating; Executing step S32: performing plasma treatment to clean the surface of the magnesium alloy wheel and perform surface modification; Execute step S33: adopt PVD process to prepare PVD high-density inorganic hybrid coating 13.

[0025] The infrared heating uses a heating power of 3.9KW and a heating time of 30s. The plasma treatment uses a power of 2KW and an Ar flow rate of 400sccm. When the PVD process is used, the background vacuum is 1.0×10 -3 Pa, process vacuum degree is 6.0×10 -1 Pa, the coating power is 10KW, the Ar flow rate is 80sccm, and O as the reaction gas 2 The flow rate is 120 sccm, and the sputtering time is 120 s. The metal target material used in the PVD process is at least one of niobium, chromium, nickel, titanium, zirconium, and tungsten, and the purity is greater than 99.95%.

[0026] In step S4, an electrostatic spraying method is used to generate a high antioxidant powder coating 14 on the outer surface of the PVD high-density inorganic hybrid coating 13, the electrostatic spraying powder amount is 60g / min, the voltage is 50KV, the static electricity is 50μA, the total gas volume is 5MPa, the baking temperature is 170°C, and the baking time is 15min.

[0027] In step S5, in order to improve the appearance and enhance the protection, a color paint 15 and a high transparent coating 16 are sequentially deposited on the outer surface of the high anti-oxidation powder coating 14. The baking temperature of the color paint 15 is 140° C. and the baking time is 20 minutes. The curing temperature of the high transparent coating 16 is 170° C. and the curing time is 15 minutes. The high transparent coating 16 is one of matte transparent powder or high gloss transparent powder.

[0028] In order to further highlight the outstanding substantial features and significant progress of the present invention, the corrosion-resistant film of the magnesium alloy wheel obtained by the method for preparing the corrosion-resistant film for the magnesium alloy wheel of the present invention was tested for corrosion resistance and wear resistance, and all the tests were qualified, as shown in Table 1.

[0029] Table 1 Corrosion resistance and wear resistance test of corrosion-resistant films for magnesium alloy wheels Test items According to the standard Testing equipment Eligibility Tape test GMW14829:2017 Slice qualified Neutral salt spray test GMW 3286: 2021, GMW 15282: 2012 (SF3600) Salt spray test chamber qualified CASS test GMW14458: 2020, GMW 15282: 2012 (DBL-240NS) Salt spray test chamber qualified Filiform trial GMW14458: 2020, GMW15287: 2018, GMW15282: 2011 (417522) Filiform Test Chamber qualified High humidity test GMW14729:2020 (ZN-L500) Condensation water test chamber qualified In summary, the method for preparing a corrosion-resistant film for a magnesium alloy wheel of the present invention is based on micro-arc oxidation technology on a magnesium alloy wheel, zirconium, titanium, iron salt, nano-silicon, and polymer resin are added to the electrolyte, and an MAO coating is generated on the surface of the magnesium alloy wheel under a constant voltage mode of an adjustable power supply, followed by chemical sealing; PVD coating is performed on the chemically sealed coating to obtain a PVD high-density inorganic hybrid coating, and physical sealing is performed to improve the adhesion and corrosion resistance between film layers; a high-oxidation resistance powder coating is sprayed on the PVD high-density inorganic hybrid coating, and the MAO coating and the chemically sealed coating are protected again, thereby obtaining a magnesium alloy wheel corrosion-resistant and wear-resistant coating with good adhesion and excellent corrosion resistance.

[0030] Those skilled in the art will appreciate that various modifications and variations may be made to the present invention without departing from the spirit or scope of the present invention. Therefore, if any modification or variation falls within the scope of protection of the appended claims and equivalents, it is considered that the present invention covers these modifications and variations.

Claims

1. A corrosion-resistant film for magnesium alloy wheels, It is characterized in that The corrosion-resistant film for magnesium alloy wheels comprises: a magnesium alloy wheel as a substrate, and a MAO coating, a chemical sealing coating, a PVD high-density inorganic hybrid coating, and a high-oxidation-resistant powder coating which are stacked from the inside to the outside in sequence, wherein: The MAO coating is an in-situ grown magnesium oxide composite coating, the magnesium oxide composite coating further contains nano zirconium, titanium, iron, and polymer resin, and the thickness of the MOA coating is 5-10 μm; The chemical sealing coating is prepared by hybridizing the MAO coating in a chromium-free sealing solution; The PVD high-density inorganic hybrid coating is a metal oxide thin film, the film thickness of the PVD high-density inorganic hybrid coating is 180-220 nm, and the metal oxide thin film contains at least one of niobium, chromium, nickel, titanium, zirconium, and tungsten; The highly anti-oxidation powder coating is prepared by using polyester resin as the resin material, carbon black as the filler, and adding a matting agent. The film thickness of the highly anti-oxidation powder coating is 80-100 μm.

2. The corrosion-resistant film for magnesium alloy wheels according to claim 1, It is characterized in that The corrosion-resistant film for magnesium alloy wheels further comprises: a color paint and a high-transparency coating sequentially deposited on the outer surface of the high-oxidation-resistant powder coating.

3. A method for preparing a corrosion-resistant film for a magnesium alloy wheel as claimed in claim 1, It is characterized in that The method for preparing the corrosion-resistant film for magnesium alloy wheels comprises: Execute step S1: Based on the micro-arc oxidation technology, zirconium, titanium, iron salt, nano silicon, and polymer resin are added to the electrolyte, and an MAO coating is generated on the surface of the magnesium alloy wheel under the constant voltage mode of the adjustable power supply, wherein the MAO coating is an in-situ grown magnesium oxide composite coating, and the magnesium oxide composite coating further contains nano zirconium, titanium, iron, and polymer resin; Executing step S2: hybridizing the MAO coating in a chromium-free sealing solution to achieve a chemically sealed coating; Executing step S3: using a PVD process to prepare a PVD high-density inorganic hybrid coating; Execute step S4: generate a high-anti-oxidation powder coating on the outer surface of the PVD high-density inorganic hybrid coating by electrostatic spraying.

4. The method for preparing the corrosion-resistant film for magnesium alloy wheels according to claim 3, It is characterized in that The method for preparing the corrosion-resistant film for magnesium alloy wheels further comprises: Execute step S5: adopt an electrostatic spraying process to deposit a color paint and a high-transparency coating on the outer surface of the high-anti-oxidation powder coating in sequence.

5. The method for preparing the corrosion-resistant film for magnesium alloy wheels according to claim 4, It is characterized in that In step S1, the voltage of the adjustable power supply in the constant voltage mode is 300 V, the corresponding process time is 7 minutes, the frequency is 500 Hz, and the duty cycle is 6%.

6. The method for preparing the corrosion-resistant film for magnesium alloy wheels according to claim 4, It is characterized in that In step S2, the MAO coating is hybridized in a chromium-free sealing solution to achieve a chemical sealing coating, and the drying temperature of the chemical sealing coating is 120° C. and the drying time is 3 minutes.

7. The method for preparing the corrosion-resistant film for magnesium alloy wheels according to claim 4, It is characterized in that In step S3, further comprising: Executing step S31: removing the attached water vapor on the surface and in the micropores of the magnesium alloy wheel by infrared heating; Executing step S32: performing plasma treatment to clean the surface of the magnesium alloy wheel and perform surface modification; Execute step S33: adopt PVD process to prepare PVD high-density inorganic hybrid coating.

8. The method for preparing the corrosion-resistant film for magnesium alloy wheels according to claim 7, It is characterized in that The heating power used for infrared heating is 3.9KW, and the heating time is 30s; the power used for plasma treatment is 2KW, and the Ar flow rate is 400sccm; when using the PVD process, the background vacuum is 1.0×10 -3 Pa, process vacuum degree is 6.0×10 -1 Pa, the coating power is 10KW, the Ar flow rate is 80sccm, and O as the reaction gas 2 The flow rate is 120 sccm and the sputtering time is 120 s. The metal target material used in the PVD process is at least one of niobium, chromium, nickel, titanium, zirconium and tungsten, and the purity is greater than 99.95%.

9. The method for preparing the corrosion-resistant film for magnesium alloy wheels according to claim 4, It is characterized in that In step S4, an electrostatic spraying method is used to generate a high antioxidant powder coating on the outer surface of the PVD high-density inorganic hybrid coating. The electrostatic spraying powder amount is 60g / min, the voltage is 50KV, the static electricity is 50μA, the total gas volume is 5MPa, the baking temperature is 170°C, and the baking time is 15min.

10. The method for preparing the corrosion-resistant film for magnesium alloy wheels according to claim 4, It is characterized in that In step S5, the baking temperature of the color paint is 140° C., and the baking time is 20 minutes; the curing temperature of the high-transparency coating is 170° C., and the curing time is 15 minutes.