Modified diamond sand line with multi-component alloy deposited on surface and preparation method of modified diamond sand line

By using tungsten, nickel and iron multi-alloy electroplating layer on the diamond sand line, the problems of short life, poor toughness and easy rust in the diamond sand line are solved, and the anti-rust effect and surface finish are improved, which is suitable for industrial production.

CN118957706APending Publication Date: 2024-11-15CHANGSHA SHARPEN ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411031676.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing diamond sand wire has a short life, poor toughness and easy rust during use, and has a poor surface finish, which affects its application effect in the cutting field.

Method used

Multi-alloys (tungsten, nickel, iron) are used as electroplating coatings. The anti-rust effect and mechanical properties are improved through the synergistic effect of tungsten and nickel, and the iron element improves the finish and bonding strength of the coating. The preparation methods include pre-plating, sanding and thickening. Electroplating steps, strictly control the metal ion concentration and process parameters.

Benefits of technology

It effectively extends the service life of diamond sand wire, improves the anti-rust effect and surface hardness, enhances the gloss and comprehensive performance of the coating, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957706A_ABST
    Figure CN118957706A_ABST
Patent Text Reader

Abstract

The invention discloses a modified diamond sand line with a multi-component alloy deposited on the surface and a preparation method of the modified diamond sand line. The preparation process of the diamond sand line comprises the following steps: cleaning a metal bus, and pre-plating the metal bus in a multi-component alloy solution to obtain a pre-plated bus; the pre-plated bus is placed in electroplating suspension liquid composed of multi-component alloy and diamond, sanding treatment is carried out, and a sand line precursor is obtained; and the sand line precursor is placed in the multi-element alloy solution again for thickening electroplating, then cleaning and drying are conducted in sequence, and the sand line is obtained. According to the sand line, based on the synergistic effect of all the components in the multi-component alloy, the bonding strength of a plating layer, the surface hardness and the anti-corrosion capacity of the sand line are greatly improved, and the problems that in the prior art, a diamond sand line is short in service life, poor in toughness, prone to corrosion and the like are effectively solved; in addition, the multi-metal coating formed by electroplating deposition can effectively improve the surface glossiness of the diamond sand line, and compared with a single metal coating, the multi-metal coating has brighter metal luster.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an alloy modified diamond sand wire, in particular to a surface deposited multi-element alloy modified diamond sand wire and a preparation method thereof, belonging to the technical field of diamond sand wire. Background Art

[0002] At present, photovoltaics, as a way of generating electricity by converting solar energy into electrical energy, has been continuously improving and perfecting in the process of social development. At the same time, solar energy, as one of the clean energy sources, is expected to replace traditional energy in the future. As an important component of photovoltaic power generation equipment, crystalline silicon is mainly cut by diamond wire cutting process. Diamond wire is often used by electrodeposition method to consolidate diamond particles on the surface of busbar substrate. It has the advantages of high strength, high cutting efficiency and good wear resistance, so it is widely used in the cutting field.

[0003] With the continuous improvement of the production process of electroplated diamond wire, there are still some defects in the existing technical solutions: due to the continuous use of diamond wire, it will rust strongly in the later practical process, affecting the service life, so improving the surface corrosion resistance of diamond wire has become one of the important factors affecting product quality; while the electroplated diamond wire is developing rapidly, corresponding requirements are also put forward for the surface finish of diamond wire, while the surface finish of diamond wire in the existing technology is poor; diamond wire must not only have a high hardness, but also must have a certain resistance to cracking during bending and deformation. Summary of the invention

[0004] In view of the problems existing in the prior art, the first purpose of the present invention is to provide a surface-deposited multi-element alloy modified diamond sand wire. The sand wire is based on the synergistic effect between the components in the multi-element alloy, which effectively solves the problems of short life, poor toughness and easy rust of diamond sand wire in the prior art. Through the synergistic effect between tungsten and nickel elements, not only can the service life of the sand wire be effectively extended, but also its anti-rust effect can be greatly improved. Through the synergistic effect between iron and nickel, while greatly improving the bonding strength between the coating and the mother wire, the surface hardness of the sand wire is further increased. In addition, the multi-element metal coating formed by electroplating deposition can also effectively improve the surface gloss of the diamond sand wire, and compared with a single metal coating, it has a brighter metallic luster.

[0005] The second object of the present invention is to provide a method for preparing surface-deposited multi-element alloy modified diamond sand wire, which strictly controls the concentration of each metal ion in the multi-element metal solution and the process parameters in each step, thereby improving the electroplating efficiency and greatly improving the comprehensive performance of the coating; further, the method has the advantages of simple process, easy operation and low cost, and is suitable for large-scale industrial production.

[0006] To achieve the above technical purpose, the present invention provides a method for preparing a surface-deposited multi-element alloy modified diamond sand wire, comprising: washing a metal busbar and placing it in a multi-element alloy solution for pre-plating to obtain a pre-plated busbar; placing the pre-plated busbar in an electroplating suspension composed of a multi-element alloy and diamond, and performing sanding treatment to obtain a sand wire precursor; placing the sand wire precursor again in a multi-element alloy solution for thickening electroplating, and then washing and drying in sequence to obtain a sand wire precursor;

[0007] The multi-component alloy solution is a metal salt solution containing tungsten, nickel and iron, wherein the concentration ratio of tungsten, nickel and iron in terms of solute is 2-10:4-16:2-12; the pH of the multi-component alloy solution is 2.5-7.

[0008] As a preferred solution, the metal busbar is at least one of stainless steel wire, high carbon steel wire and tungsten wire. More preferably, the metal busbar is tungsten wire.

[0009] As a preferred solution, the multi-element alloy solution further includes 30-80 g / L of sodium citrate and 5-40 g / L of boric acid.

[0010] As a preferred solution, the cleaning process of the metal busbar is as follows: after laying out the metal busbar, the metal busbar is placed in a cleaning solution at 30 to 80° C. for cleaning for 10 to 60 minutes, and then immersed in anhydrous ethanol for 1 to 5 minutes.

[0011] As a preferred solution, the cleaning liquid is a 20-60 g / L sodium hydroxide solution.

[0012] As a preferred solution, during the pre-plating process, the concentration of iron salt in the multi-alloy solution is 20-100 g / L as ferrous sulfate, the concentration of nickel salt is 40-150 g / L as nickel sulfamate, and the concentration of tungsten salt is 30-70 g / L as sodium tungstate.

[0013] As a preferred solution, during the sanding process, the concentration of iron salt in the multi-element alloy solution is 30-110 g / L as ferrous sulfate, the concentration of nickel salt is 50-160 g / L as nickel sulfamate, and the concentration of tungsten salt is 30-100 g / L as sodium tungstate.

[0014] As a preferred solution, during the thickening electroplating process, the concentration of iron salt in the multi-element alloy solution is 60-160 g / L as ferrous sulfate, the concentration of nickel salt is 40-90 g / L as nickel sulfamate, and the concentration of tungsten salt is 40-90 g / L as sodium tungstate.

[0015] As a preferred solution, the particle size of the diamond is 5 to 35 μm; the diameter of the metal busbar is 50 to 155 μm.

[0016] As a preferred solution, the conditions of the pre-plating process are: pH value 2.6-7.0, temperature 30-65°C, current density 4-15A / dm 2 , pre-plating time 3 to 10 seconds.

[0017] As a preferred solution, the conditions of the sanding process are: pH value 3-7.0, temperature 40-70°C, current density 12-25A / dm 2 , sanding time is 3 to 10 seconds.

[0018] As a preferred solution, the conditions of the thickening electroplating process are: pH value 3.5-7.0, temperature 40-70°C, current density 15-30A / dm 2 , sanding time is 3 to 10 seconds.

[0019] The present invention also provides a surface-deposited multi-element alloy modified diamond sand wire, which is obtained by any one of the above-mentioned preparation methods.

[0020] The main mechanism of action of the technical solution provided by the present invention is: tungsten element itself has excellent service life of rust-proof agent, and tungsten solute entering into the alloy matrix will induce solid solution strengthening effect, increase interatomic bonding and diffusion activation energy, and improve the mechanical properties of the overall alloy material; nickel, as the main element, has the characteristics of good corrosion resistance, high electroplating efficiency and good surface finish. At the same time, the FCC crystal structure of nickel element has more slip systems, which can effectively alleviate the internal stress caused by electroplating on the surface of thin tungsten wire with large curvature. The addition of iron element will make the precipitation potential deviation in the electroplating process larger, which is easy to cause polarization phenomenon near the cathode, which will be conducive to obtaining an overall coating with finer grains and better surface quality.

[0021] Compared with the prior art, the beneficial technical effects of the technical solution of the present invention are:

[0022] 1) The diamond abrasive wire provided by the present invention is based on the synergistic effect between the components in the multi-component alloy, which effectively solves the problems of short life, poor toughness and easy rust of the diamond abrasive wire in the prior art. The synergistic effect between tungsten and nickel elements can not only effectively extend the service life of the abrasive wire, but also greatly improve its anti-rust effect. The synergistic effect between iron and nickel can greatly improve the surface quality of the coating and further increase the electroplating efficiency. In addition, the multi-metal coating formed by electroplating deposition can also effectively improve the surface gloss of the diamond abrasive wire, and has a brighter metallic luster compared with a single metal coating.

[0023] 2) In the preparation method provided by the present invention, by strictly controlling the concentration of each metal ion in the multi-metal solution and the process parameters in each step, the electroplating efficiency is improved while the comprehensive performance of the coating is greatly improved. This method has the advantages of simple process, easy operation and low cost, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a flow chart of the method for preparing diamond abrasive wire in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments is described clearly and completely below, and the following embodiments are used to illustrate the present invention. Changes or modifications known to those skilled in the art are also included in the protection scope of the present invention.

[0026] Example 1

[0027] like Figure 1 As shown, the method for preparing the diamond wire provided in this embodiment comprises the following steps:

[0028] S1: Pretreatment: After laying out the busbar, it is first placed in a cleaning solution at 45°C and then soaked in anhydrous ethanol for 5 minutes;

[0029] S2: Pre-plating: Take the cleaned busbar substrate and place it in the electroplating solution for pre-plating, add 25g / L ferrous sulfate, 65g / L nickel sulfamate, 30g / L sodium tungstate, 40g / L sodium citrate, and 6g / L boric acid, mix, adjust the pH value to 4.0, and the temperature to 45°C to obtain a pre-plated busbar;

[0030] S3: Sanding: After pre-plating, the busbar is placed in a diamond suspension electroplating solution, and 35 g / L ferrous sulfate, 70 g / L nickel sulfamate, 35 g / L sodium tungstate, 45 g / L sodium citrate, and 8 g / L boric acid are added and mixed, and the pH value is adjusted to 4.4 and the temperature is 45°C. Diamond particles are compositely sanded to the pre-plated surface of the busbar substrate to obtain a diamond sand wire;

[0031] S5: Thickening: Place the diamond wire in a thickening plating solution, add 40g / L ferrous sulfate, 75g / L nickel sulfamate, 40g / L sodium tungstate, 50g / L sodium citrate, and 10g / L boric acid, mix, adjust the pH value to 4.7, the temperature to 45°C, and deposit a coating on the outer layer;

[0032] S6: Post-processing: The obtained diamond wire is cleaned in pure water and then dried.

[0033] In a specific implementation, the busbar substrate is tungsten wire, the cleaning solution is 40 g / L NaOH, the cleaning time is 25 min, the temperature is 45° C., and the busbar substrate diameter is 141 μm.

[0034] Furthermore, the current density of the pre-plating step is 8A / dm 2 , pre-plating time 5s, current density of the sanding step 12A / dm 2 , sanding time 8s; current density of the thickening step 15A / dm 2 , thickening time is 10s, the particle size of the diamond is 20-30μm, and the median diameter is 25μm; the drying temperature of the diamond wire is 120℃, and the drying time is 5min.

[0035] Example 2

[0036] The method for preparing the diamond wire provided in this embodiment comprises the following steps:

[0037] S1: Pretreatment: After laying out the busbar, it is first placed in a cleaning solution at a temperature of 50°C; then soaked in anhydrous ethanol for 3 minutes;

[0038] S2: Pre-plating: Take the cleaned busbar substrate and place it in the electroplating solution for pre-plating, add 30g / L ferrous sulfate, 75g / L nickel sulfamate, 30g / L sodium tungstate, 45g / L sodium citrate, and 8g / L boric acid, mix, adjust the pH value to 4.2, and the temperature to 48°C to obtain a pre-plated busbar;

[0039] S3: Sanding: After pre-plating, the busbar is placed in a diamond suspension electroplating solution, and 40 g / L ferrous sulfate, 85 g / L nickel sulfamate, 40 g / L sodium tungstate, 50 g / L sodium citrate, and 12 g / L boric acid are added and mixed, and the pH value is adjusted to 4.8 and the temperature is 50°C. Diamond particles are compositely sanded to the pre-plated surface of the busbar substrate to obtain a diamond sand wire;

[0040] S5: Thickening: Place the diamond wire in a thickening plating solution, add 45g / L ferrous sulfate, 95g / L nickel sulfamate, 45g / L sodium tungstate, 55g / L sodium citrate, and 15g / L boric acid, mix, adjust the pH value to 5.0, the temperature to 55°C, and deposit a coating on the outer layer;

[0041] S6: Post-processing: The obtained diamond wire is cleaned in pure water and then dried.

[0042] Example 3

[0043] like Figure 1 As shown, a preparation process of electroplated tungsten, nickel, and iron alloy diamond wire includes the following steps:

[0044] S1: Pretreatment: After laying out the busbar, it is first placed in a cleaning solution at 60°C; then soaked in anhydrous ethanol for 2 minutes;

[0045] S2: Pre-plating: Take the cleaned busbar substrate and place it in the electroplating solution for pre-plating, add 35g / L ferrous sulfate, 80g / L nickel sulfamate, 35g / L sodium tungstate, 48g / L sodium citrate, and 10g / L boric acid, mix, adjust the pH value to 4.4, and the temperature to 50°C to obtain a pre-plated busbar;

[0046] S3: Sanding: After pre-plating, the busbar is placed in a diamond suspension electroplating solution, and 45 g / L ferrous sulfate, 90 g / L nickel sulfamate, 45 g / L sodium tungstate, 52 g / L sodium citrate, and 13 g / L boric acid are added and mixed, and the pH value is adjusted to 4.9 and the temperature is 55°C. Diamond particles are compositely sanded to the pre-plated surface of the busbar substrate to obtain a diamond sand wire;

[0047] S5: Thickening: Place the diamond wire in a thickening plating solution, add 50 g / L ferrous sulfate, 100 g / L nickel sulfamate, 50 g / L sodium tungstate, 55 g / L sodium citrate, and 15 g / L boric acid, mix, adjust the pH value to 5.2, the temperature to 58°C, and deposit a coating on the outer layer;

[0048] S6: Post-processing: The obtained diamond wire is cleaned in pure water and then dried.

[0049] Comparative Example 1

[0050] S1: Pretreatment: After laying out the busbar, it is first placed in a cleaning solution at 45°C and then soaked in anhydrous ethanol for 5 minutes;

[0051] S2: Pre-plating: Take the cleaned busbar substrate and place it in the electroplating solution for pre-plating, add 80g / L of nickel sulfamate and 5g / L of boric acid to mix, adjust the pH value to 3.9, and the temperature to 45°C to obtain a pre-plated busbar;

[0052] S3: Sanding: After pre-plating, the busbar is placed in a diamond suspension electroplating solution, and 90 g / L of nickel sulfamate and 10 g / L of boric acid are added to mix, the pH value is adjusted to 4.3, the temperature is 50°C, and diamond particles are compositely sanded to the pre-plated surface of the busbar substrate to obtain a diamond sand wire;

[0053] S5: Thickening: Place the diamond wire in a thickening plating solution, add 100 g / L nickel sulfamate and 15 g / L boric acid, mix, adjust the pH value to 5.2, the temperature to 55°C, and deposit a coating on the outer layer;

[0054] S6: Post-processing: The obtained diamond wire is cleaned in pure water and then dried.

[0055] Comparative Example 2

[0056] S1: Pretreatment: After laying out the busbar, it is first placed in a cleaning solution at 60°C; then soaked in anhydrous ethanol for 2 minutes;

[0057] S2: Pre-plating: Take the cleaned busbar substrate and place it in the electroplating solution for pre-plating, add 50g / L ferrous sulfate and 10g / L boric acid to mix, adjust the pH value to 3.4, and the temperature to 45°C to obtain a pre-plated busbar;

[0058] S3: Sanding: After pre-plating, the busbar is placed in a diamond suspension electroplating solution, and 60 g / L of ferrous sulfate and 15 g / L of boric acid are added to mix, the pH value is adjusted to 3.6, the temperature is 50°C, and diamond particles are compositely sanded to the pre-plated surface of the busbar substrate to obtain a diamond sand wire;

[0059] S5: Thickening: Place the diamond wire in a thickening plating solution, add 70 g / L ferrous sulfate and 20 g / L boric acid to mix, adjust the pH value to 3.8, the temperature to 52°C, and deposit a coating on the outer layer;

[0060] S6: Post-processing: The obtained diamond wire is cleaned in pure water and then dried.

[0061] The diamond wires in the above three embodiments and two comparative examples were taken out to make samples, and the data of their durability and bonding strength are shown in Table 1 respectively.

[0062] Durability: Prepare a sample with a length of 170 mm and use it to cut a flat glass with a thickness of 5 mm until the sample fails. Definition of failure: The number of diamond particles per unit area is less than 10; Durability index: Cutting area (mm 2 ) = cutting depth (mm) * material thickness (mm);

[0063] Bonding strength: Take a diamond wire sample and clamp it between two nylon rods with a diameter of 20 mm. Bend the wire back and forth around the outer diameter of the nylon rod until the coating is basically peeled off. The number of bends is defined as the bonding condition of the coating. The average number of bends of 5 samples is taken as the number of bends of the sample.

[0064] Table 1

[0065] <![CDATA[Durability (mm 2 )]]> Bonding strength (times) Example 1 291 77 Example 2 279 84 Example 3 288 90 Comparative Example 1 224 48 Comparative Example 2 218 46

[0066] The diamond wires in the above three embodiments and two comparative examples were taken out to prepare samples, and the data of their anti-rust effects and appearances are shown in Table 2.

[0067] Anti-rust effect: The neutral salt spray method is used to test the anti-rust of the coating. The test solution is sodium chloride, which is continuously sprayed on the surface of the sample. After the test, the surface salt deposits are gently washed with running cold water and then dried. Test indicators: Determined by the proportion of rust area per unit area, rust rate (%) = rust area (%) / total unit area (%)

[0068] Appearance: Direct qualitative evaluation of the surface finish under a stereo microscope.

[0069] Table 2

[0070] Anti-rust effect (%) Appearance Example 1 2 bright Example 2 11 Brighter Example 3 27 bright Comparative Example 1 75 Brighter Comparative Example 2 59 Dark

[0071] From the data in Table 1 and Table 2, we can see that:

[0072] Compared with traditional nickel and iron coatings, the diamond wire prepared by the present invention using tungsten, iron and nickel alloy coatings has significantly improved durability, bonding strength and rust prevention effect; at the same time, compared with iron plating, tungsten, iron and nickel plating can obtain better surface finish.

Claims

1. A method for preparing a surface-deposited multi-element alloy modified diamond sand wire, characterized in that: After cleaning the metal busbar, the busbar is placed in a multi-element alloy solution for pre-plating to obtain a pre-plated busbar; the pre-plated busbar is placed in an electroplating suspension composed of a multi-element alloy and diamond, and sanded to obtain a sand wire precursor; the sand wire precursor is placed in the multi-element alloy solution again for thickening electroplating, and then washed and dried in sequence to obtain; The multi-component alloy solution is a metal salt solution containing tungsten, nickel and iron, wherein the concentration ratio of tungsten, nickel and iron in terms of solute is 2-10:4-16:2-12; the pH of the multi-component alloy solution is 2.5-7.

2. The method for preparing a surface-deposited multi-element alloy modified diamond sand wire according to claim 1, characterized in that: The metal busbar is at least one of stainless steel wire, high carbon steel wire and tungsten wire; the multi-element alloy solution also includes 30-80 g / L of sodium citrate and 5-40 g / L of boric acid.

3. The method for preparing a surface-deposited multi-element alloy modified diamond sand wire according to claim 2, characterized in that: During the pre-plating process, the concentration of the iron salt in the multi-element alloy solution is 20-100 g / L as ferrous sulfate, the concentration of the nickel salt is 40-150 g / L as nickel sulfamate, and the concentration of the tungsten salt is 30-70 g / L as sodium tungstate.

4. The method for preparing a surface-deposited multi-element alloy modified diamond sand wire according to claim 2, characterized in that: During the sanding process, the concentration of iron salt in the multi-element alloy solution is 30-110 g / L as ferrous sulfate, the concentration of nickel salt is 50-160 g / L as nickel sulfamate, and the concentration of tungsten salt is 30-100 g / L as sodium tungstate.

5. The method for preparing a surface-deposited multi-element alloy modified diamond sand wire according to claim 2, characterized in that: In the thickening electroplating process, the concentration of iron salt in the multi-element alloy solution is 60-160 g / L as ferrous sulfate, the concentration of nickel salt is 40-90 g / L as nickel sulfamate, and the concentration of tungsten salt is 40-90 g / L as sodium tungstate.

6. The method for preparing a surface-deposited multi-element alloy modified diamond sand wire according to claim 1, characterized in that: The particle size of the diamond is 5 to 35 μm; the diameter of the metal busbar is 50 to 155 μm.

7. The method for preparing a surface-deposited multi-element alloy modified diamond wire according to any one of claims 1 to 6, characterized in that: The conditions of the pre-plating process are: pH value 2.6-7.0, temperature 30-65°C, current density 4-15A / dm 2 , pre-plating time 3 to 10 seconds.

8. The method for preparing a surface-deposited multi-element alloy modified diamond wire according to any one of claims 1 to 6, characterized in that: The conditions of the sanding process are: pH value 3-7.0, temperature 40-70°C, current density 12-25A / dm 2 , sanding time is 3 to 10 seconds.

9. The method for preparing a surface-deposited multi-element alloy modified diamond wire according to any one of claims 1 to 6, characterized in that: The conditions of the thickening electroplating process are: pH value 3.5-7.0, temperature 40-70°C, current density 15-30A / dm 2 , sanding time is 3 to 10 seconds.

10. A surface deposited multi-element alloy modified diamond sand wire, characterized in that: Obtained by the preparation method according to any one of claims 1 to 9.