Step splicing type eddy current testing reference block and crack simulation method
Through the step-stage eddy current detection comparison test block and crack simulation method, the problem of large opening width of artificial defects in the prior art is solved, more accurate crack simulation and detection results are achieved, and the processing and metrology process is simplified.
Patent Information
- Application Number
- CN202411041630.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The artificial defect opening of the existing eddy current detection test block is large in width, and it is impossible to effectively simulate the tiny gap of natural cracks, resulting in inaccurate detection results.
The step-stage eddy current detection comparison test block and crack simulation method are used to form multiple simulated cracks by splicing two sizing pieces together to form each other, which is used to detect surface open defects and buried defects, and to simulate closed and open cracks.
A narrower artificial defect opening gap is achieved, which can more accurately simulate natural cracks, improve the accuracy of detection results, and simplify the processing and metrology process.
Smart Images

Figure CN118961354A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nondestructive testing, and in particular to a step-jointed eddy current testing comparison test block and a crack simulation method. Background Art
[0002] Eddy current testing is a non-destructive testing technology commonly used in the aerospace industry. In recent years, it has also been widely used in rail transportation, energy and electricity, nuclear power, automobiles, petroleum and petrochemicals, and special equipment industries. Eddy current testing uses defects to cause changes in the electromagnetic properties of materials to discover, locate, and quantify defects. Like other non-destructive testing methods, eddy current testing also requires the use of test blocks with known artificial defects to debug the detection system and set the sensitivity. Therefore, whether the artificial defects of the comparison test block can well simulate natural defects has an important impact on the eddy current testing results.
[0003] The objects of eddy current testing are mainly surface and near-surface crack defects. Therefore, the artificial defects of the comparison test block are also mainly simulated by cracks. Usually the opening gap of the crack is very small, so it is hoped that the opening width of the artificial defect is as narrow as possible while ensuring the dimensional accuracy, so as to be as similar to the actual crack as possible.
[0004] The artificial defects of existing eddy current test blocks are mainly grooves, which are generally processed by wire cutting or EDM. The grooves on the upper and lower surfaces can be directly processed by wire cutting or EDM. For buried grooves, a hole is usually drilled in the middle of the location where the groove is required to pass through the conductive molybdenum wire, and then the groove is cut upward and downward by EDM to form the groove of the required height. Affected by the size of the EDM electrode and the wire cutting molybdenum wire, the minimum groove width that can be produced by these two processing technologies is about 0.13mm , The opening width of the groove-type artificial defects obtained by the above-mentioned processing technology is relatively large, and it is not possible to simulate the tiny gap of the natural crack well, resulting in inaccurate detection results. Moreover, the smaller the defect, the greater the deviation between the artificial groove and the actual crack morphology, and the greater the deviation of the detection result. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems in the prior art and to provide a step-jointed eddy current detection comparison test block and a crack simulation method.
[0006] One of the purposes of the present invention is to provide a step-jointed eddy current detection comparison test block, comprising a first joint block and a second joint block, wherein the first joint block and the second joint block both have a joint surface, and the joint surfaces of the first joint block and the second joint block are provided with a plurality of step structures along their length directions, and after the first joint block and the second joint block are joined together, the plurality of step structures are joined together to form a plurality of simulated cracks, wherein the simulated cracks formed by the vertical joint surfaces of the plurality of step structures are used for eddy current detection sensitivity calibration of surface opening defects and buried defects and weld penetration measurement calibration.
[0007] As a public manner, two vertical joint surfaces of the mutually jointed step structures of the first joint block and the second joint block are in direct contact, which is used to simulate a closed crack.
[0008] As a public method, an insulating film is provided between two vertical joint surfaces of the step structure of the first joint block and the second joint block to simulate an open crack.
[0009] At least one of the two vertical joint surfaces of the mutually jointed step structure of the first joint block and the second joint block is sprayed with an insulating paint layer to simulate an open crack.
[0010] As a disclosed manner, the two vertical joining surfaces of the mutually joined step structures of the first joining block and the second joining block are vertical joining surfaces or inclined joining surfaces.
[0011] As a public method, the paint spraying surface selects the side where the step surface is convex.
[0012] As a disclosed method, the shallowest step of the first assembly block corresponds to the thinnest covering surface of the second assembly block, and a reinforcing structure is provided outside the thinnest covering surface of the second assembly block.
[0013] As a disclosed manner, a plurality of step structures constitute gradient steps.
[0014] As another object of the present invention, a crack simulation method for the above-mentioned step-jointed eddy current testing comparison test block is provided, comprising the following steps:
[0015] Select two test blocks made of the same material or with similar electromagnetic properties as the workpiece to be tested as the comparison test blocks;
[0016] Making a step structure on the joint surface of the two joint test blocks, and each joint test block has a plurality of steps on the joint surface;
[0017] The multiple step surfaces of the two assembled test blocks can be assembled to form multiple simulated cracks.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention provides a new artificial defect design method and designs a new test block structure. This method uses two vertically spliced facades that match in size and contact each other to replace the groove as an artificial defect. The opening gap of the artificial defect can be made narrower, and the buried artificial defect is easier to make. It can simulate closed cracks and open cracks.
[0020] The present invention designs a new step-jointed eddy current comparison test block by utilizing the above method. The new test block has the advantages of compact structure, wide range of simulated defect types, reasonable setting of artificial defect size, simpler processing and measurement, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the structure of the first splicing block according to an embodiment of the present invention.
[0022] Figure 2 Schematic diagram of the structure of the second splicing block according to an embodiment of the present invention.
[0023] Figure 3 The figure is a schematic diagram of the structure after the first splicing block and the second splicing block are spliced together according to an embodiment of the present invention.
[0024] Figure 4 Schematic diagram of the detection area of the first detection surface according to an embodiment of the present invention.
[0025] Figure 5 Schematic diagram of the detection area of the second detection surface according to an embodiment of the present invention.
[0026] Figure 6 Schematic diagram of three types of crack defects in the present invention.
[0027] Description of reference numerals:
[0028] 1. The first assembly block, 2. The second assembly block, 3. Step structure, 4. Simulated cracks, 5. Strengthened structure. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Unless otherwise defined, the technical terms or scientific terms used herein shall have the usual meanings understood by persons of ordinary skill in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. Words such as "include" or "comprise" and the like mean that the elements or objects appearing before "include" or "comprise" cover the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. Words such as "connect" or "connected" and the like are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0031] The eddy current flow direction in the conductor is parallel to the detection surface, and defects perpendicular to the eddy current flow direction will cause eddy current field distortion. Therefore, eddy current detection has better detection efficiency for defects perpendicular to the detection surface, while layered defects parallel to the surface have no effect on eddy current detection. Based on this principle, two step-shaped blocks of matching sizes can be assembled together to form a whole. The horizontal surface of the step has no effect on the detection, and the vertical surface can be used to simulate defects perpendicular to the detection surface.
[0032] It should be noted that the width of the defect, i.e. the vertical gap, which is perpendicular to the direction of eddy current flow, will affect the distribution of the electromagnetic field between the metal and the gap, so the width of the vertical gap affects the eddy current detection results. However, for horizontal thin layer gaps, when their horizontal size is larger than the eddy current influence area, the change in their horizontal size does not affect the distribution of eddy current between the metal and the gap. Therefore, the cracks formed on the horizontal joint surfaces of the multiple step structures 3 of the present invention have no effect on the eddy current detection results. The simulated cracks 4 formed by the vertical joint surfaces of the multiple step structures 3 of the present invention can make the crack width narrower, thereby solving the problem that the opening width of artificial defects such as grooves is large and cannot simulate the tiny gaps of natural cracks well, resulting in inaccurate detection results.
[0033] The present embodiment provides a step-joined eddy current detection comparison test block, including a first joint block 1 and a second joint block 2, wherein the first joint block 1 and the second joint block 2 have a joint surface, and the joint surfaces of the first joint block 1 and the second joint block 2 are provided with a plurality of step structures 3 along their length direction, and the plurality of step structures 3 can form a continuous gradient step, and after the first joint block 1 and the second joint block 2 are joined together, the plurality of step structures 3 are joined together to form a plurality of simulated cracks 4, wherein the simulated cracks 4 formed by the vertical joint surfaces of the plurality of step structures are used for eddy current detection sensitivity calibration of surface opening defects and buried defects and weld penetration measurement calibration of laser welding or electron beam welding, such as Figure 6 shown.
[0034] As a preferred embodiment, the two vertical joint surfaces of the mutually jointed step structures 3 of the first joint block 1 and the second joint block 2 are in direct contact, so as to simulate a closed crack.
[0035] As a preferred embodiment, an insulating film is provided between two vertical joint surfaces of the step structures 3 of the first joint block 1 and the second joint block 2 to simulate an open crack.
[0036] As a preferred embodiment, at least one of the two vertical joint surfaces of the mutually jointed step structure 3 of the first joint block 1 and the second joint block 2 is sprayed with an insulating paint layer to simulate an open crack.
[0037] As a preferred embodiment, the two vertical joint surfaces of the mutually assembled step structure 3 of the first joint block 1 and the second joint block 2 are vertical joint surfaces or inclined joint surfaces. When the joint surfaces are inclined joint surfaces, the inclined joint surfaces can simulate inclined cracks, and the vertical joint surfaces at the ends can be used to simulate cracks with varying depths.
[0038] As a preferred embodiment, the step surface of the painted surface is selected as the convex side, which can prevent the rounding of the paint layer at the concave corner due to surface tension from causing the increase of the gap between the parts.
[0039] As a preferred embodiment, the shallowest step of the first assembly block 1 corresponds to the thinnest covering surface of the second assembly block 2, and a reinforcement structure is provided outside the thinnest covering surface of the second assembly block.
[0040] This embodiment also provides a crack simulation method for the above-mentioned step-jointed eddy current testing comparison test block, comprising the following steps:
[0041] Select two test blocks made of the same material or with similar electromagnetic properties as the workpiece to be tested as the comparison test blocks;
[0042] Making a step structure on the joint surface of the two joint test blocks, and each joint test block has a plurality of steps on the joint surface;
[0043] The multiple step surfaces of the two assembled test blocks can be assembled to form multiple simulated cracks.
[0044] The test block design method of the present invention has the following advantages: it can simulate narrower cracks, which are closer to the actual test object; it can simulate closed cracks and open cracks, and has a wide range of applications; the same method can be used to simulate buried cracks without the need for other processing methods such as drilling.
[0045] The following is a description in the form of specific embodiments.
[0046] In this embodiment, the design of the first splicing block 1 and the second splicing block 2 is as follows:
[0047] Select materials with the same or similar electromagnetic properties as the workpiece to be tested;
[0048] Use this material to make Figure 1-Figure 2 The two test blocks with step structure joint surfaces shown, namely the first joint block 1 and the second joint block 2, each of which has a plurality of steps, and the distances between each step surface and the detection surface are h1, h2, h3...hn respectively;
[0049] For example, h1 can be between 0.3-0.8mm, h2 can be twice h1, h3 can be three times h1...hn can be n times h1. The above values meet the conventional needs of the industry. Currently, the most common shallow crack depth in the industry is 0.5mm. Some special industries have higher requirements, and the shallowest crack depth may be 0.2mm. The distance between multiple step surfaces and the detection surface can be increased exponentially after 0.2mm according to the above value principle.
[0050] Preferably, since the thickness of the h1 part is usually thin, in order to maintain structural stability and facilitate fixation, a thicker reinforcing structure can be added to the side of the h1 part, and the thickness of the corresponding position of the other test block is reduced to achieve splicing;
[0051] The first assembly block 1 and the second assembly block 2 are assembled to form a new test block with a total thickness of T. The assembled test block is as follows: Figure 3 As shown;
[0052] The assembled test block has two upper and lower test surfaces, each with three usable test areas. Figure 4 and Figure 5 ;
[0053] When testing on the first test surface:
[0054] The first detection surface area 1, the first detection surface area 1, is the detection surface surface opening defect, and its own height is h1, h2, h3...hn;
[0055] Zone 2 of the first detection surface is a buried defect with no openings on the upper and lower surfaces, with a buried depth of h1 and a height of h2-h1, a buried depth of h2 and a height of h3-h2, and finally a buried depth of hn-1 and a height of hn-hn-1.
[0056] Zone 3 of the first detection surface is a surface opening defect far from the detection surface, and the buried depths from the detection surface are h1, h2...hn respectively;
[0057] Turn the assembled test block 180 degrees left and right, and test it on the second test surface:
[0058] The second detection surface area 1 is a surface opening defect far away from the detection surface, and the buried depths from the detection surface are T-hn, T-hn-1...T-h1 respectively;
[0059] The second detection surface area 2 is a buried defect with no openings on the upper and lower surfaces, with a buried depth of T-hn, a height of hn-hn-1, a buried depth of T-hn-1, a height of hn-1-hn-2, etc.
[0060] The second detection surface area 3 is the open defects on the detection surface, and their heights are T-hn, T-hn-1...T-h1 respectively;
[0061] The spliced test block of the present invention has a compact structure and rich artificial defect types. A spliced test block has two detection surfaces, six detection areas, and three types of defects; and the defect size is reasonably set, and the sizes of various defects are distributed in a step-by-step manner, which is convenient for equipment debugging; the spliced test block of the present invention is easy to process, the size is easier to control, and the size measurement is also simpler.
[0062] More specifically, the first assembly block 1 and the second assembly block 2 are made of 7075 aluminum alloy and are manufactured by mechanical processing.
[0063] The first assembly block 1 and the second assembly block 2 are both 240 mm long, 80 mm wide, and 5.5 mm high. The heights of h1 to h5 are 0.5, 1.0, 1.5, 2.0, and 2.5 mm respectively.
[0064] The thickness of the left reinforced part of the second assembly block 2 is 2.5 mm, and the thickness of the corresponding part of the first assembly block 1 is 3.0 mm.
[0065] Each step plane is a 40×40mm rectangle, the left reinforced area is 20×40mm, and the rightmost step is extended by 20mm to set up a fixing mechanism.
[0066] The dimensions of the test block after assembly are 240 mm long, 120 mm wide and 5.5 mm high.
[0067] Areas 6-10 of the first detection surface 1 are detection surface opening defects, and their own heights are 0.5mm, 1.0mm, 1.5mm, 2.0mm and 2.5mm respectively.
[0068] The first detection surface 2 areas 11-14 are all buried defects with a height of 0.5 mm and buried depths of 0.5 mm, 1.0 mm, 1.5 mm and 2.0 mm respectively.
[0069] The first detection surface 3 zones 15-19 are open defects far from the detection surface side, and the buried depths from the detection surface are 0.5 mm, 1.0 mm, 1.5 mm, 2.0 mm and 2.5 mm respectively.
[0070] The second detection surface 1 area 20-24 is an open defect far away from the detection surface side, and the buried depths from the detection surface are 3.0 mm, 3.5 mm, 4.0 mm, 4.5 mm and 5.0 mm respectively.
[0071] The second detection surface 2 areas 25-28 are all buried defects with a height of 0.5 mm and buried depths of 3.0 mm, 3.5 mm, 4.0 mm and 4.5 mm respectively.
[0072] The second detection surface 3 zones 29-33 are detection surface opening defects, and their own heights are 3.0 mm, 3.5 mm, 4.0 mm, 4.5 mm and 5.0 mm respectively.
[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A step-jointed eddy current test comparison block, characterized in that: The invention comprises a first assembly block (1) and a second assembly block (2), wherein the first assembly block (1) and the second assembly block (2) are both provided with an assembly surface for being assembled with each other, and the assembly surfaces of the first assembly block (1) and the second assembly block (2) both include a plurality of step structures (3). After the assembly surfaces of the first assembly block (1) and the second assembly block (2) are assembled, the plurality of step structures (3) are assembled to form a plurality of simulated cracks (4), wherein the simulated cracks (4) formed by the vertical assembly surfaces of the plurality of step structures (3) are used for eddy current detection sensitivity calibration.
2. The step-jointed eddy current testing comparison test block according to claim 1, characterized in that: The two vertical joint surfaces of the mutually jointed step structures (3) of the first joint block (1) and the second joint block (2) are in direct contact, so as to simulate a closed crack.
3. The step-jointed eddy current testing comparison test block according to claim 1, characterized in that: An insulating film is provided between two vertical joint surfaces of the mutually jointed step structures (3) of the first joint block (1) and the second joint block (2) to simulate an open crack.
4. The step-jointed eddy current testing comparison test block according to claim 1, characterized in that: At least one of the two vertical joint surfaces of the mutually jointed step structure (3) of the first joint block (1) and the second joint block (2) is sprayed with an insulating paint layer to simulate an open crack.
5. The step-jointed eddy current testing comparison test block according to claim 4, characterized in that: The paint spraying surface selects the side where the step surface is the convex surface.
6. The step-jointed eddy current testing comparison test block according to claim 1, characterized in that: The two vertical joining surfaces of the mutually joined step structures (3) of the first joining block (1) and the second joining block (2) are vertical joining surfaces or inclined joining surfaces.
7. The step-jointed eddy current testing comparison test block according to claim 1, characterized in that: The materials of the first assembly block (1) and the second assembly block (2) are the same as or have similar electromagnetic properties to the workpiece to be inspected.
8. The step-jointed eddy current testing comparison test block according to claim 1, characterized in that: The shallowest step of the first assembly block (1) corresponds to the thinnest covering surface of the second assembly block (2), and a reinforcing structure (5) is provided outside the thinnest covering surface of the second assembly block (2).
9. The step-jointed eddy current testing comparison test block according to claim 1, characterized in that: A plurality of step structures (3) constitute gradient steps.
10. The crack simulation method of the step-jointed eddy current testing comparison test block according to claim 1, characterized in that: The following steps are involved: Select two test blocks made of the same material or with similar electromagnetic properties as the workpiece to be tested as the comparison test blocks; Making a step structure on the joint surface of the two joint test blocks, and each joint test block has a plurality of steps on the joint surface; The multiple step surfaces of the two assembled test blocks can be assembled to form multiple simulated cracks.