Preparation method of integrally formed inductor
By using a method for fabricating integrally molded inductors, the shortcomings of traditional inductors in terms of high integration, heat dissipation performance, and production efficiency are overcome, achieving stability and reliability in high-frequency and high-power applications, and adapting to the design requirements of different electronic devices.
Patent Information
- Application Number
- CN202411305798.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional inductors have significant shortcomings in terms of high integration, heat dissipation performance, production efficiency, and high-frequency, high-power applications, making it difficult to meet the compact design and high-performance requirements of modern electronic devices.
The method of fabricating an integrally molded inductor involves using a mosaic layout mold and injection molding technology to integrally press magnetic powder and coil into shape, designing heat dissipation grooves, and improving the conductivity of the electrodes through laser processing and electroplating, thereby simplifying the production process.
It improves the integration and heat dissipation performance of the inductor, enhances the conductivity and mechanical strength of the inductor, simplifies the manufacturing process, adapts to different application scenarios with flexibility, and ensures the stability and reliability of the inductor under high frequency and high power conditions.
Smart Images

Figure CN118969477A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of inductor manufacturing, and in particular to a method for preparing an integrally formed inductor. Background Art
[0002] As an important component of electronic components, inductors are widely used in power management, signal processing, energy storage and other fields, especially in high-frequency and high-current circuit design. With the improvement of the performance and integration of electronic equipment, the demand for inductor products is also growing, especially in the design of graphics processing units (GPUs), central processing units (CPUs) and power modules, the application of inductors is particularly important.
[0003] Limitations of Traditional Inductors
[0004] Traditional inductors are usually made of discrete components or laminated processes. Typical ferrite inductors are made by sintering ferrite materials. Although this type of inductor performs well in medium and low frequency applications, it has obvious limitations in the following aspects:
[0005] Large size and low integration: Traditional inductors are large in size and difficult to meet the needs of high integration and miniaturization. With the strict requirements of modern electronic devices on volume and space, traditional inductors are gradually unable to adapt to compact design requirements.
[0006] Limited power density: For high-power applications, traditional ferrite inductors have large losses when large currents pass through them, making it difficult to achieve efficient heat dissipation, which can easily cause the inductor to overheat and affect the stability of the circuit.
[0007] Poor heat dissipation performance: Due to design limitations, traditional inductors have fewer heat dissipation channels. Especially in high power density applications, heat accumulation can easily lead to component overheating and failure.
[0008] Low production efficiency: The manufacturing process of traditional inductors often requires multiple steps and manual operations, which has low production efficiency and requires multiple discrete components to be arranged side by side, increasing the complexity of production.
[0009] Advantages of One-Piece Molded Inductors
[0010] In order to overcome the shortcomings of traditional inductors, one-piece molded inductors have emerged. Unlike discrete inductors, one-piece molded inductors use powder metallurgy technology to directly mold magnetic powder and coils together through injection molding. Compared with traditional laminated processes, one-piece molded inductors have the following advantages:
[0011] High integration: The one-piece molded inductor presses the coil and the magnetic core into one piece, avoiding the space waste of discrete components and is suitable for miniaturized and high-density integrated circuit design.
[0012] Excellent heat dissipation performance: In the structure of the one-piece molded inductor, heat dissipation grooves can be designed between each inductor unit. This design greatly increases the heat dissipation surface area of the inductor, effectively reduces the operating temperature, and improves the reliability of the inductor.
[0013] Flexible design: The preparation method of this inductor can flexibly adjust the number and shape of the inductor row to meet different application requirements. At the same time, through laser processing and electroplating, the size and quality of the electrode can be accurately controlled to improve the conductivity of the inductor.
[0014] Simplified production process: The one-piece molded inductor adopts mold injection molding and automated technology, which simplifies the production process, not only improves production efficiency, but also reduces the complexity of manual intervention. There is no need to configure different fixtures for different inductor rows, which greatly reduces the difficulty of production management.
[0015] Requirements for high frequency and high power applications
[0016] With the rapid development of semiconductor technology, inductors are gaining more and more attention in high-frequency and high-power applications. Especially in 5G communications, IoT devices, consumer electronics, and new energy fields, electronic devices have put forward higher requirements for high power density and low loss of inductors. In order to meet these requirements, inductor devices must not only have high current handling capabilities, but also maintain stable inductance values in high-frequency environments. At the same time, heat dissipation performance and volume have also become key factors in the design.
[0017] At present, the ferrite inductors on the market can no longer meet these high-performance requirements, especially in miniaturization and high-frequency applications, their performance is obviously insufficient. Therefore, developing an integrated molded inductor with high power density, excellent heat dissipation performance and suitable for high-frequency applications has become an important research direction in the inductor industry. Summary of the invention
[0018] The purpose of the present invention is to provide a method for preparing an integrally formed inductor in view of the shortcomings of the prior art, so as to solve the problems raised in the background technology.
[0019] To achieve the above object, the present invention provides the following technical solution: a method for preparing an integrally formed inductor, comprising the following steps:
[0020] S1: Prepare a pit mold with a mosaic layout, with 4-40 square pits arranged in the length and width directions of the mold, and the mold is divided into an upper mold and a lower mold, and the specifications of the two are the same;
[0021] S2: injecting the injection molding powder into the upper mold through the feeding hole, pressing at a mold temperature of 180-200°C and a pressure of 5-20MPa for 2-4 seconds, and demolding to obtain the inductor blank;
[0022] S3: Use flat copper wire to wind a "J"-shaped coil, and place it on the lower mold filled with injection molding powder;
[0023] S4: Cover the upper mold on the lower mold where the coil is placed, leaving a distance of 1 mm between the two molds, and press again with the injection molding material to obtain a full-plate blank;
[0024] S5: spraying epoxy resin on the surface of the blank, and baking and curing at 160-200° C. for 30 minutes;
[0025] S6: cutting along the edge of the block according to the number of required parallel inductors to obtain small pieces of inductor blanks;
[0026] S7: spraying transparent epoxy resin on the surface of the small inductor blank obtained in S6, and then baking at 160-200° C. for 30 minutes under nitrogen protection to cure, completely wrapping the surface of the component and covering the exposed electrodes and cuts;
[0027] S8: Use laser to burn out the terminal, and then electroplate the terminal to obtain the finished inductor.
[0028] As a preferred technical solution of the present invention, the injection molding powder is composed of a mixture of soft magnetic alloy powder, amorphous powder and carbonyl iron powder, the mass proportion of the soft magnetic alloy powder or amorphous powder is 20% to 60%, and the mass proportion of the carbonyl iron powder is 40% to 80%, wherein the particle diameter D50 of the soft magnetic alloy powder or amorphous powder is 10-30μm, and the particle diameter D50 of the carbonyl iron powder is 4-8μm.
[0029] As a preferred technical solution of the present invention, the injection molding material also includes a thermoplastic organic matter, which is selected from polypropylene (PP), polycarbonate (PC), polystyrene (PS) or polyethylene (PE), and is mixed with the magnetic powder in a ratio of 5:1 to 10:1, and a plasticizer dibutyl phthalate or butyl formate is added in an amount of 1% of the total mass of the magnetic powder.
[0030] As a preferred technical solution of the present invention, the steps of preparing the injection molding powder include:
[0031] S21: Mix the soft magnetic alloy powder, amorphous powder, carbonyl iron powder with polypropylene, polycarbonate, polystyrene or polyethylene in proportion, add plasticizer dibutyl phthalate or butyl formate, and send them into an internal mixer for uniform internal mixing;
[0032] S22: repeatedly kneading the kneaded coarse material to fully mix the magnetic powder and the thermoplastic organic matter into a large block;
[0033] S23: putting the bulk material into a reciprocating pelletizer and squeezing it into short cylindrical pellets through a screen;
[0034] S24: Use a vibrating screen to sieve out particles of 30-60 mesh as materials for injection molding.
[0035] As a preferred technical solution of the present invention, the width of the flat copper wire is 1 / 3 to 1 / 5 of the width of the mold pit, and the thickness is 1 / 10 to 1 / 15 of the width.
[0036] As a preferred technical solution of the present invention, the remaining part of the inductor row after cutting can be further cut into single inductors of different sizes and inductance values.
[0037] As a preferred technical solution of the present invention, the insulating layer of the end of the inductor is removed by laser technology, and the electrode position is automatically identified by a camera, laser ablation is used to expose the electrode, and electroplating is performed on the exposed area of the electrode to form a tin layer, the thickness of which is 50-100μm higher than the surface of the insulating layer.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] 1. Improve production efficiency and flexibility: By using mosaic layout molds and injection molding technology, the present invention can mold multiple inductor units at one time, simplifying the multi-step process of traditional inductor manufacturing. There is no need to frequently adjust the mold or prepare additional fixtures during the production process, which greatly improves production efficiency. At the same time, the number and shape of the inductor row can be flexibly adjusted according to demand to adapt to different application scenarios, reducing the complexity of production management.
[0040] 2. Excellent heat dissipation performance: There are heat dissipation grooves between each inductor unit, which greatly increases the heat dissipation surface area and effectively solves the problem of heat accumulation in high-power inductors during operation. After epoxy resin spraying and secondary curing, the inductor has better heat dissipation and high temperature resistance, ensuring the long-term stability of the inductor under high current or high frequency applications, and avoiding performance degradation or failure due to overheating.
[0041] 3. Improve the performance and reliability of the inductor: High-precision laser ablation technology is used to ensure the precise size of the electrode at the exposed part of the inductor end, and the conductivity is improved through the electroplating process to ensure the low loss characteristics of the inductor. This design not only enhances the electrical performance of the inductor, but also improves the mechanical strength and durability of the component, enabling it to work stably for a long time under high frequency and high power conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic diagram of the local structure of the mold;
[0043] Figure 2 This is a schematic diagram of the mold after it is filled with plastic powder;
[0044] Figure 3It is a schematic diagram of the position relationship between the coil and the mold;
[0045] Figure 4 This is a schematic diagram of the inductor after demoulding;
[0046] Figure 5 This is a schematic diagram of the inductor after cutting. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings and multiple embodiments.
[0049] Example 1: Preparation of conventional power inductor
[0050] S1: Mold preparation
[0051] See also Figure 1 and Figure 2 The mold is designed with a standard mosaic layout, the number of pits is set to 20, and the length-to-width ratio of the pits is 1:1. The mold is designed with an upper mold and a lower mold. The material of the mold is high-strength steel to ensure that it can withstand a pressure of 5-20MPa during the pressing process. The pit size of the mold is about 5mm x 5mm and the depth is 3mm, which is suitable for the preparation of conventional inductors.
[0052] S2: Injection material preparation
[0053] The following raw materials are used to prepare the injection molding powder:
[0054] Soft magnetic alloy powder (50%, D50 = 20 μm)
[0055] Carbonyl iron powder (50%, D50=6μm)
[0056] The thermoplastic matrix material is polypropylene (PP), mixed with magnetic powder in a ratio of 7:1
[0057] Plasticizer dibutyl phthalate, added at 1% of the mass of magnetic powder
[0058] All materials are mixed evenly in an internal mixer, and after kneading and forming, large blocks are formed, which are then put into a reciprocating granulator with a screen aperture of 300μm to finally obtain granules of 30-60 mesh. After screening, the granules are stored for later use.
[0059] S3: Coil Winding
[0060] See also Figure 3 , a flat copper wire with a width of 1.5mm and a thickness of 0.15mm is used, and it is wound into a "J" shape on a winding mold. During winding, it is necessary to ensure that the spacing between turns is uniform and the shape of the wound coil matches the mold pit.
[0061] S4: Suppression
[0062] The coil is placed on the pit of the lower mold, ensuring that the coil fits tightly to the bottom of the mold. Subsequently, the upper mold is covered on the lower mold, leaving a 1mm gap between the molds. The injection molding material is injected into the upper mold, and pressed at a mold temperature of 180-200℃ and a pressure of 10MPa for 2-4 seconds. After completion, the mold is demolded to obtain a preliminarily formed inductor blank.
[0063] S5: Epoxy spraying and initial curing
[0064] Spray the epoxy resin evenly on the surface of the blank to ensure that the surface of each inductor unit is completely covered. Put the blank into the oven and bake it at 160℃ for 30 minutes to solidify the epoxy resin and form a protective layer.
[0065] S6: Cutting the inductor blank
[0066] See also Figure 4 and Figure 5 , use the cutting tool to cut along the edge of the inductor unit to cut into the required side-by-side inductors or individual inductor units. The cutting gap between each inductor is controlled within 0.5mm to ensure dimensional accuracy.
[0067] S7: Secondary spraying and curing
[0068] Transparent epoxy resin was sprayed evenly on the surface of each inductor unit again, especially on the cut edges and exposed electrode parts, and then baked again at 160℃ under nitrogen protection for 30 minutes to ensure that the component surface was completely covered and the electrodes and cuts were covered.
[0069] S8: Laser tip processing and electroplating
[0070] Laser technology is used to remove the insulating layer at the end of the inductor, and a camera is used to automatically identify the location of the electrode, and the electrode area is exposed through precise laser cutting. Subsequently, the component is placed in an electroplating bath, and tin electroplating technology is used to form a 50-100μm thick tin layer on the end to ensure the electrical performance and mechanical strength of the inductor.
[0071] Example 2: Preparation of high power density inductor
[0072] S1: Mold preparation
[0073] See also Figure 1 and Figure 2 For high-power applications, the mold is designed with smaller pits. There are 40 pits on the mold, and the aspect ratio of the pits is 1:2. The mold is made of high-strength hardened steel to withstand higher pressing pressure. The size of the pit is 2.5mm x 5mm and the depth is 4mm, which is suitable for the production of high-current inductors.
[0074] S2: Injection material preparation
[0075] The injection molding powder adopts the following formula:
[0076] Soft magnetic alloy powder (accounting for 60%, D50=15μm)
[0077] Carbonyl iron powder (40%, D50 = 4 μm)
[0078] The base material is polycarbonate (PC), mixed with magnetic powder in a ratio of 6:1
[0079] The plasticizer is butyl formate, added at 1% of the total mass of the magnetic powder
[0080] All materials are mixed evenly in an internal mixer to form large blocks. Subsequently, the blocks are put into a reciprocating pelletizer for kneading and squeezed through a 200μm screen to form short cylindrical particles to obtain 40-80 mesh particles. The screened particles are used for injection molding of high-power inductors.
[0081] S3: Wide copper wire winding
[0082] See also Figure 3 In order to adapt to high current inductance, a wider flat copper wire is used. The copper wire width is 1 / 3 of the pit width (about 1.67mm), and the thickness is 1 / 12 of the pit width (about 0.2mm). The coil is wound in a tight "J" shape to ensure the best inductance performance when current is conducted.
[0083] S4: Suppression
[0084] Place the coil in the pit of the lower mold to ensure that the coil fits flatly. The upper mold covers the lower mold, leaving a gap of 0.5mm. The injection molding material is pressed under high temperature and high pressure (200℃, 20MPa) for 2 seconds. After completion, demolding is completed to obtain a high-power inductor blank.
[0085] S5: Thickened epoxy spray
[0086] Spray thickened epoxy resin on the surface of the inductor body, spray two layers to ensure the heat dissipation capacity of the inductor under high power. The baking temperature is increased to 180℃ and the time is extended to 40 minutes to ensure that the epoxy resin is fully cured.
[0087] S6: Cutting and finishing
[0088] See also Figure 4 and Figure 5 According to the required number of inductors, the inductor units are accurately cut along the cutting line. The gap between the inductors is controlled within 0.2mm during cutting. After cutting, the inductors are arranged neatly.
[0089] S7: Full coating and secondary curing
[0090] Spray transparent epoxy resin for the second time to ensure that the surface and edges of the inductor are completely covered. Perform a curing treatment at 180°C again to ensure that the inductor will not break down under high current load.
[0091] S8: Laser end treatment and thickening electroplating
[0092] The insulating layer at the end of the inductor is ablated by laser technology, and the electrode is automatically identified and accurately cut to expose the electrode. Then, tin electroplating is carried out in the electroplating bath, and the thickness of the tin layer is 80-120μm, ensuring that the inductor has good conductivity under high current.
[0093] Example 3: Preparation of small-size high-frequency inductor
[0094] S1: Small mold design
[0095] The mold is designed for small-size inductors, with a pit size of 2mm x 2mm and a pit depth of 2mm, which is suitable for making small inductors for high-frequency (above 1MHz) applications. There are 10 pits arranged in the mold with an aspect ratio of 1:1.
[0096] S2: Preparation of injection molding materials
[0097] The injection molding material adopts the following formula:
[0098] Amorphous powder (40%, D50 = 20 μm)
[0099] Carbonyl iron powder (accounting for 60%, D50=5μm)
[0100] Polystyrene (PS) is used as the matrix material and mixed with magnetic powder in a ratio of 8:1.
[0101] Dibutyl phthalate is a plasticizer, added at 1% of the mass of the magnetic powder
[0102] After mixing, it is kneaded and squeezed to form a large block, and then passed through a reciprocating granulator to screen out 50-80 mesh particles to ensure that it is suitable for high-frequency inductors.
[0103] S3: Thin copper wire winding
[0104] A thinner flat copper wire is used, the width of the copper wire is 1 / 5 of the pit (about 0.4mm), and the thickness is 1 / 15 (about 0.13mm). Automatic winding equipment is used to wind the coil into a "J" shape with a high number of turns to increase the inductance value of the high-frequency inductor.
[0105] S4: Pressing and preliminary forming
[0106] The coil was placed in the lower mold, covering the upper mold with a gap of 1 mm. The mold temperature was 200°C and the pressure was 15 MPa, and then the mold was demolded after 2 seconds to obtain a preliminary inductor blank.
[0107] S5-S8: Subsequent processes
[0108] Epoxy spraying, cutting, secondary spraying and laser end treatment are carried out according to standard procedures to ensure that the inductor has good conductivity and heat dissipation performance under high frequency conditions.
[0109] Example 4: Preparation of multi-unit parallel inductors
[0110] S1: Special mold design
[0111] The mold is arranged with 30 pits, the aspect ratio of the pits is 1:3, and a 1mm groove is reserved between each pit to increase the heat dissipation performance of the inductor row. The pit size is 4mm x 4mm and the depth is 3mm, which is suitable for making multi-unit parallel inductors.
[0112] S2: Preparation of powder for large-scale injection molding
[0113] The proportion of injection molding powder is:
[0114] Soft magnetic alloy powder (40%, D50 = 30 μm)
[0115] Amorphous powder (30%, D50 = 25 μm)
[0116] Carbonyl iron powder (30%, D50=6μm)
[0117] The base material is polyethylene (PE), mixed with magnetic powder in a ratio of 5:1
[0118] Through the reciprocating pelletizer and screener, 30-60 mesh pellets are produced for mass injection molding.
[0119] S3: Multi-unit coil winding
[0120] Copper wire is used to wind multiple coils at the same time, and a coil is placed independently in each pit. The width and thickness of the coil are adjusted according to the size of the pit to ensure that each inductor unit has a consistent inductance value.
[0121] S4-S8: Standard process
[0122] After standard injection molding, epoxy resin spraying, cutting, secondary curing and laser end treatment, multiple parallel inductor units are obtained. Finally, single inductors or multiple parallel inductors can be cut according to needs, and the remaining parts can be reprocessed or sold.
[0123] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in the field. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an integrally formed inductor, characterized in that: The following steps are involved: S1: Prepare a pit mold with a mosaic layout, with 4-40 square pits arranged in the length and width directions of the mold, and the mold is divided into an upper mold and a lower mold, and the specifications of the two are the same; S2: injecting the injection molding powder into the upper mold through the feeding hole, pressing at a mold temperature of 180-200°C and a pressure of 5-20MPa for 2-4 seconds, and demolding to obtain the inductor blank; S3: Use flat copper wire to wind a "J"-shaped coil, and place it on the lower mold filled with injection molding powder; S4: Cover the upper mold on the lower mold where the coil is placed, leaving a distance of 1 mm between the two molds, and press again with the injection molding material to obtain a full-plate blank; S5: spraying epoxy resin on the surface of the blank, and baking and curing at 160-200° C. for 30 minutes; S6: cutting along the edge of the block according to the number of required parallel inductors to obtain small pieces of inductor blanks; S7: spraying transparent epoxy resin on the surface of the small inductor blank obtained in S6, and then baking at 160-200° C. for 30 minutes under nitrogen protection to cure, completely wrapping the surface of the component and covering the exposed electrodes and cuts; S8: Use laser to burn out the terminal, and then electroplate the terminal to obtain a finished inductor.
2. The method for preparing an integrally formed inductor according to claim 1, characterized in that: The injection molding powder is composed of a mixture of soft magnetic alloy powder, amorphous powder and carbonyl iron powder, the mass proportion of the soft magnetic alloy powder or amorphous powder is 20% to 60%, the mass proportion of the carbonyl iron powder is 40% to 80%, wherein the particle diameter D50 of the soft magnetic alloy powder or amorphous powder is 10-30μm, and the particle diameter D50 of the carbonyl iron powder is 4-8μm.
3. The method for preparing an integrally formed inductor according to claim 2, characterized in that: The injection molding material also includes a thermoplastic organic matter, which is selected from polypropylene (PP), polycarbonate (PC), polystyrene (PS) or polyethylene (PE), and is mixed with the magnetic powder in a ratio of 5:1 to 10:1, and a plasticizer dibutyl phthalate or butyl formate is added in an amount of 1% of the total mass of the magnetic powder.
4. The method for preparing an integrally formed inductor according to claim 3, characterized in that: The steps of preparing the injection molding powder include: S21: Mix the soft magnetic alloy powder, amorphous powder, carbonyl iron powder with polypropylene, polycarbonate, polystyrene or polyethylene in proportion, add plasticizer dibutyl phthalate or butyl formate, and send them into an internal mixer for uniform internal mixing; S22: repeatedly kneading the kneaded coarse material to fully mix the magnetic powder and the thermoplastic organic matter into a large block; S23: putting the bulk material into a reciprocating pelletizer and squeezing it into short cylindrical pellets through a screen; S24: Use a vibrating screen to sieve out particles of 30-60 mesh as materials for injection molding.
5. The method for preparing an integrally formed inductor according to claim 1, characterized in that: The width of the flat copper wire is 1 / 3 to 1 / 5 of the width of the mold pit, and the thickness is 1 / 10 to 1 / 15 of the width.
6. The preparation method according to claim 1, characterized in that: The remaining part of the inductor row after cutting can be further cut into single inductors of different sizes and inductance values.
7. The preparation method according to claim 1, characterized in that: The insulating layer at the end of the inductor is removed by laser technology, and the electrode position is automatically identified by a camera. Laser ablation is used to expose the electrode, and electroplating is performed on the exposed area of the electrode to form a tin layer with a thickness of 50-100μm higher than the surface of the insulating layer.
Citation Information
Cited By
Preparation method of copper-magnetic co-fired inductor and copper-magnetic co-fired inductor
CN119993720A