Complementary bipolar device preparation method based on bonding process
The preparation of complementary bipolar devices through bonding process on SOI silicon wafers is solved, and the complex problem of epitaxial processes in the prior art is achieved, and the efficient preparation of complementary bipolar transistors with high collector breakdown voltage and low collector series resistance is achieved.
Patent Information
- Application Number
- CN202410989737.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
AI Technical Summary
The existing complementary bipolar device processing requires epitaxial processes, resulting in complex and inefficient processes, making it difficult to achieve device preparation with high collector breakdown voltage and low collector series resistance without using epitaxial processes.
Using a bonding process method, N-type and P-type buried layers are prepared by lithography and ion implantation on SOI silicon wafers, and bonded to the double-throwing silicon wafer with oxide layer. After debonding, the substrate silicon is separated. , combined with MEMS manufacturing technology, a dielectric isolation groove and contact hole were prepared on the N-type top silicon to form a complementary bipolar transistor.
The process flow is simplified, the device preparation efficiency is improved, and complementary bipolar transistors with high collector breakdown voltage and low collector series resistance are prepared without the use of epitaxial processes.
Smart Images

Figure CN118969712A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor integrated circuits, and in particular to a method for preparing a complementary bipolar device based on a bonding process. Background Art
[0002] The complementary bipolar process uses a technology similar to the NPN bipolar process to obtain a very symmetrical vertical PNP transistor, so that NPN and PNP transistors with complementary performance can be obtained in the same IC (Integrated Circuit), and it is compatible with JFET devices. It has a combination of the best performance required by high-speed operational amplifiers, such as large bandwidth, high input impedance, low bias current, low noise, low power consumption, wide output range, large output current and low distortion.
[0003] The mainstream complementary bipolar device processing is to first prepare a buried layer on a substrate silicon wafer, and then perform an epitaxial growth process on the surface of the silicon wafer. The transistor processed in this way has a high collector breakdown voltage and a low collector series resistance. The present invention provides a new method for preparing a complementary bipolar transistor, which can also achieve a collector breakdown voltage and a low collector series resistance without using an epitaxial process. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a complementary bipolar device based on a bonding process, which method can complete the preparation of the complementary bipolar device by omitting the epitaxial process, thereby improving the preparation efficiency of the device.
[0005] It adopts the following technical solutions: A method for preparing a complementary bipolar device based on a bonding process comprises the following steps: S1, take an SOI silicon wafer, and use photolithography and ion implantation processes to complete the preparation of an N-type buried layer and a P-type buried layer in a specific area of the N-type top silicon of the SOI silicon wafer; S2, take a double-polished silicon wafer with an oxide layer and bond it to the N-type top silicon of the SOI silicon wafer using a bonding process; S3, using a debonding process to separate the substrate silicon and the N-type top silicon of the SOI silicon wafer, so that the bottom side of the N-type top silicon is exposed; S4, preparing a dielectric isolation groove on the N-type top silicon by oxidation, film formation, photolithography, dielectric etching, deep silicon etching, sidewall oxidation, polysilicon filling and annealing, CMP planarization, hot phosphoric acid etching and oxide layer etching processes; S5, forming an N-type buried layer connection region in the N-type top silicon by photolithography, phosphorus implantation and ion diffusion process; forming a P-type buried layer connection region and a P well in the N-type top silicon by photolithography, boron implantation and diffusion process; S6, forming a P-type base region on the N-type top silicon by implanting boron and ion diffusion process; forming an N-type base region in the P well by implanting phosphorus and diffusion process; S7, forming an N-type emitter region in the P-type base region by implanting phosphorus; forming a P-type emitter region in the N-type base region by implanting boron; S8, depositing an oxide layer on the entire surface of the N-type top silicon to form an interlayer dielectric layer; S9, completing the preparation of contact holes in the collector region, base region and emitter region of the transistor through photolithography, etching and corrosion processes; S10. Finally, the final electrode is prepared through metal sputtering, photolithography and etching processes.
[0006] Furthermore, in step S1, a silicon oxide film is grown on the surface of the N-type top silicon of the SOI silicon wafer.
[0007] Compared with the prior art, the present invention has the following beneficial effects: The present invention forms N-type and P-type buried layers by performing an implantation and annealing process on the top silicon of an SOI silicon wafer, then bonds one side of the top silicon wafer to another oxidized silicon wafer, removes the substrate silicon of the original SOI silicon wafer by debonding, and thus forms an SOI silicon wafer with a buried layer on the remaining silicon wafer, and completes the preparation of a complementary bipolar transistor double buried layer without using an epitaxial process by combining semiconductor manufacturing technology and MEMS manufacturing technology, thereby simplifying the process flow and improving the preparation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 is a schematic diagram of the structure of the SOI silicon wafer in step S1 of the present invention; Figure 2 is a schematic diagram of step S1 of the present invention; Figure 3 is a schematic diagram of step S2 of the present invention; Figure 4 is a schematic diagram of step S3 of the present invention; Figure 5 is a schematic diagram of step S4 of the present invention; Figure 6 is a schematic diagram of step S5 of the present invention; Figure 7 is a schematic diagram of step S6 of the present invention; Figure 8 is a schematic diagram of step S7 of the present invention; Fig. 9 is a schematic diagram of step S8 of the present invention; Fig.10 is a schematic diagram of step S9 of the present invention; Fig.11 It is a schematic diagram of step S10 of the present invention.
[0009] Explanation of the reference numerals: 100, SOI silicon wafer; 101, N-type top silicon; 102, substrate silicon; 103, insulating layer; 104, silicon oxide film; 200, double-polished silicon wafer; 201, oxide layer; 1, P-type buried layer; 2, N-type buried layer; 3, dielectric isolation groove; 4, N-type buried layer connection area; 5, P-type buried layer connection area; 6, P well; 7, P-type base region; 8, N-type base region; 9, N-type emitter region; 10, P-type emitter region; 11, interlayer dielectric layer; 12, contact hole; 13, electrode. DETAILED DESCRIPTION
[0010] To make the present invention more clear, a method for preparing a complementary bipolar device based on a bonding process of the present invention is further described below in conjunction with the accompanying drawings. The specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0011] A method for preparing a complementary bipolar device based on a bonding process comprises the following steps: S1, such as Figure 1 As shown, a SOI silicon wafer 100 is taken, and the SOI silicon wafer 100 has an N-type top silicon 101 on the upper side, a substrate silicon 102 on the lower side, and an insulating layer 103 located between the N-type top silicon 101 and the substrate silicon 102; a silicon oxide film 104 is grown on the surface of the N-type top silicon 101 by using a thermal oxidation method; Figure 2 As shown, the P-type buried layer 1 and the N-type buried layer 2 are prepared in a specific area of the N-type top silicon 101 by photolithography and ion implantation processes; wherein the P-type buried layer 1 and the N-type buried layer 2 do not contact each other.
[0012] S2, such as Figure 3 As shown, a double-polished silicon wafer 200 is taken, and the upper and lower surfaces of the double-polished silicon wafer 200 have an oxide layer 201 formed after thermal oxidation; the double-polished silicon wafer 200 is connected to the N-type top silicon 101 of the SOI silicon wafer 100 through silicon-silicon bonding using a bonding process.
[0013] S3, such as Figure 4 As shown, the debonding process is used to separate the substrate silicon 102 and the N-type top silicon 101 of the SOI silicon wafer 100, so that the bottom side of the N-type top silicon 101 is exposed, so that the buried layer (P-type buried layer 1, N-type buried layer 2) is transferred from the surface of the N-type top silicon 101 to its bottom, completing the buried layer preparation.
[0014] S4, such as Figure 5As shown, a termination layer (not shown in the figure) is first formed on the surface of the N-type top silicon 101 by thermal oxidation and deposition of silicon nitride, and then deep trench etching is completed by dielectric trench lithography, dielectric etching, deep silicon etching and degumming processes. Finally, a dielectric isolation trench 3 is prepared on the N-type top silicon 101 by sidewall oxidation, polysilicon filling and annealing, CMP flattening, hot phosphoric acid etching and oxide layer etching processes. The dielectric isolation trench 3 isolates the P-type buried layer 1 and the N-type buried layer 2.
[0015] S5, such as Figure 6 As shown, an N-type buried connection region 4 is formed in the N-type top silicon 101 by photolithography, phosphorus implantation and ion diffusion processes; a P-type buried connection region 5 and a P-well 6 are formed in the N-type top silicon 101 by photolithography, boron implantation and diffusion processes, and the P-type buried connection region 5 is located in the P-well 6.
[0016] S6, such as Figure 7 As shown, a P-type base region 7 is formed on the N-type top silicon 101 by implanting boron and ion diffusion process, and the P-type base region 7 is not in contact with the N-type buried layer connection region 4; an N-type base region 8 is formed in the P well 6 by implanting phosphorus and ion diffusion process.
[0017] S7, such as Figure 8 As shown, an N-type emitter region 9 is formed in the P-type base region 7 by implanting phosphorus; and a P-type emitter region 10 is formed in the N-type base region 8 by implanting boron.
[0018] S8, such as Fig. 9 As shown, an oxide layer is deposited on the entire surface of the N-type top silicon 101 (the other surface relative to the buried layer) to form an interlayer dielectric layer 11.
[0019] S9, such as Fig.10 As shown, the contact holes 12 of the collector region, base region and emitter region of the transistor are prepared by photolithography, etching and corrosion processes; S10, such as Fig.11 As shown, the final electrode 13 is finally prepared through metal sputtering, photolithography, and etching processes to complete the preparation of the complementary bipolar device.
[0020] Through the manufacturing method of the present invention, the semiconductor manufacturing technology and the MEMS manufacturing technology are combined to complete the preparation of the double buried layer of the complementary bipolar transistor without using the epitaxial process; the process flow is simplified as a whole, and the manufacturing efficiency is improved.
[0021] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention.
Claims
1. A method for preparing a complementary bipolar device based on a bonding process, characterized in that: The following steps are involved: S1, taking an SOI silicon wafer (100), and using photolithography and ion implantation processes to complete the preparation of a P-type buried layer (1) and an N-type buried layer (2) in a specific area of an N-type top silicon layer (101) of the SOI silicon wafer (100); S2, taking a double-polished silicon wafer (200) with an oxide layer, and bonding it to the N-type top silicon (101) of the SOI silicon wafer (100) by using a bonding process; S3, using a debonding process to separate the substrate silicon (102) and the N-type top silicon (101) of the SOI silicon wafer (100), so that the bottom side of the N-type top silicon (101) is exposed; S4, preparing a dielectric isolation groove (3) on the N-type top silicon (101) by oxidation, film formation, photolithography, dielectric etching, deep silicon etching, sidewall oxidation, polysilicon filling and annealing, CMP planarization, hot phosphoric acid etching and oxide layer etching processes; S5, forming an N-type buried layer connection region (4) in the N-type top silicon (101) by photolithography, phosphorus implantation and ion diffusion processes; forming a P-type buried layer connection region (5) and a P well (6) in the N-type top silicon (101) by photolithography, boron implantation and diffusion processes; S6, forming a P-type base region (7) on the N-type top silicon (101) by implanting boron and performing an ion diffusion process; and forming an N-type base region (8) in the P well (6) by implanting phosphorus and performing a diffusion process; S7, forming an N-type emitter region (9) by implanting phosphorus into the P-type base region (7); and forming a P-type emitter region (10) by implanting boron into the N-type base region (8); S8, depositing an oxide layer on the entire surface of the N-type top silicon (101) to form an interlayer dielectric layer (11); S9, completing the preparation of contact holes (12) in the collector region, base region and emitter region of the transistor by photolithography, etching and corrosion processes; S10. Finally, the final electrode (13) is prepared by metal sputtering, photolithography, and etching processes.
2. The method for preparing a complementary bipolar device based on a bonding process according to claim 1, characterized in that: In step S1, a silicon oxide film (104) is grown on the surface of the N-type top silicon layer (101) of the SOI silicon wafer (100).
Citation Information
Cited By
Monolithic integration structure of dielectric isolation bipolar IC and piezoresistive MEMS device
CN121269614A
Monolithic integrated structure for dielectrically isolated bipolar IC and piezoresistive MEMS devices
CN121269614B