Transverse gallium nitride-based varactor structure and preparation method thereof

By introducing a transverse structure and multiple PN junction diodes in parallel in the gallium nitride-based variable container, the problems of small varactor range and high process difficulty in the vertical structure are solved, and a larger varactor range and high current density are achieved. Other GaN RF device processes.

CN118969859AInactive Publication Date: 2024-11-15XIDIAN UNIV +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411043247.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing gallium nitride-based varactor diode devices have problems such as small varactor range, high process difficulty and inability to fully reflect material advantages in vertical structures, especially in radio frequency circuits with insufficient tuning and frequency modulation performance.

Method used

Adopting a transverse gallium nitride-based variable container structure, the P-type region is set to form a transverse PN junction with two-dimensional electronic gas to achieve pressurized variable capacity, and the variable capacity of the variable capacitor is improved through parallel connection of multiple anode and cathode electrodes. Range, compatible with other gallium nitride RF device processes.

Benefits of technology

It achieves a larger varactor range and high current density, avoids the defects of the vertical structure, and is compatible with mainstream gallium nitride RF device processes for easy preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969859A_ABST
    Figure CN118969859A_ABST
Patent Text Reader

Abstract

The transverse gallium nitride-based varactor structure sequentially comprises a substrate layer, a composite buffer layer, a channel layer, a barrier layer and a passivation layer from bottom to top, a plurality of grooves are formed in the barrier layer and the channel layer, the bottom ends of the grooves penetrate through the barrier layer to the upper middle portion of the channel layer, negative electrodes are arranged in the grooves, and positive electrodes are arranged in the rest grooves. A P-type injection region is arranged on one side, close to the positive electrode, in the groove provided with the positive electrode; the preparation method comprises the following steps: firstly cleaning the substrate layer, sequentially growing the composite buffer layer, the composite channel layer and the barrier layer on the substrate layer, then forming a plurality of P-type regions from part of the barrier layer to part of the channel layer, then etching the barrier layer to the middle upper part of the channel layer by utilizing an etching technology to form a plurality of grooves, respectively growing the negative electrode and the positive electrode in the grooves, and finally forming the P-type regions on the substrate layer. And finally depositing a passivation layer. According to the invention, the parallel connection of a plurality of variable capacitance diodes is realized on the transverse gallium nitride-based heterojunction structure, and the variable capacitance device has the characteristics of large variable capacitance range and compatibility with a gallium nitride-based radio frequency device process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of semiconductor devices, and in particular relates to a lateral gallium nitride-based varactor structure and a preparation method thereof. Background Art

[0002] Gallium nitride (GaN) stands out in the preparation of high-performance microwave devices with its larger bandgap, higher critical breakdown electric field and higher electron saturation drift velocity, as well as excellent physical and chemical properties such as stable chemical properties, high temperature resistance and radiation resistance, and has great application potential. With its development and application in monolithic integrated circuits (MMICs), active and passive devices based on gallium nitride are increasingly gaining public attention. As a key device in microwave integrated circuits, variable capacitors determine their important position in gallium nitride-based devices. Usually, variable capacitor devices based on GaN are mainly varactor diodes, and their most significant feature is that the capacitance value can be adjusted by changing the reverse bias voltage. This makes it very useful in circuits that require dynamic adjustment of capacitance. Varactor diodes are particularly suitable for high-frequency circuits such as wireless communications and radio frequency applications. It can be used to tune radio frequency signals and achieve precise frequency control, which is essential for equipment such as radio receivers and transmitters.

[0003] At present, there have been many reports on vertical structures in GaN-based varactor diode devices, but the advantages of GaN cannot be reflected in the vertical structure, and the process difficulty of GaN vertical structure is greater than that of lateral structure. Secondly, because the varactor diode plays the role of tuning and frequency modulation in the RF circuit, its capacitance change range is very important. In addition, with the compression of chip size, higher requirements are also placed on the device design and layout design of the chip. In order to simplify the design, using the same varactor device to achieve a larger capacitance range is also one of the research focuses in the field of RF devices.

[0004] Patent application CN108198758A proposes a method for manufacturing a vertically structured gallium nitride power diode device, which adopts the following steps: step 1, providing a substrate and an epitaxial layer on the substrate; step 2, providing a patterned epitaxial layer surface and etching grooves; step 3, depositing a first anode metal on the surface of the epitaxial layer between the grooves; step 4, covering the second anode metal in the groove and on the surface of the first layer of anode metal; step 5, making a cathode on the back of the device. The invention can improve the forward output current and reverse blocking voltage of the device, and improve the device performance of the gallium nitride power diode; however, due to the large bandgap width of GaN, the advantages of critical breakdown electric field strength and stable chemical properties cannot be reflected in the vertical structure, and it has the disadvantage of a small variable capacitance range. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a lateral gallium nitride-based varactor structure and a preparation method thereof, by setting a plurality of P-type regions to form a lateral PN junction with a two-dimensional electron gas, so as to achieve pressurized variable capacitance; in the present invention, a plurality of anode electrodes and a plurality of cathode electrodes are set, and when pressurized, the plurality of anode electrodes are pressurized together to achieve parallel connection of multiple diodes, thereby improving the variable capacitance range of the variable capacitor; at the same time, the present invention can achieve compatibility with other gallium nitride radio frequency device processes, and is easy to prepare.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A lateral gallium nitride-based variable capacitor structure comprises, from bottom to top, a substrate layer 1, a composite buffer layer 2, a composite channel layer 3 and a barrier layer 4; a heterojunction is formed between the composite channel layer 3 and the barrier layer 4, and the heterojunction polarization forms a two-dimensional electron gas on one side of the composite channel layer 3; a plurality of grooves are arranged on the barrier layer 4 and part of the composite channel layer 3, and the bottom ends of the grooves penetrate the barrier layer 4 and the two-dimensional electron gas to the middle and upper part of the composite channel layer 3; a cathode electrode 6 is arranged in part of the grooves, and an anode electrode 7 is arranged in the remaining grooves, and a P-type injection region 8 is arranged on the side close to the anode electrode in the groove where the anode electrode 7 is arranged; the P-type injection region 8 respectively forms a PN junction with the barrier layer 4 and part of the channel layer 3 on the side close to the cathode electrode 6, and the PN junction and the cathode electrode 6 are respectively connected with the anode electrode 7 to form a PN junction diode, and the capacitance of the PN junction diode changes when pressure is applied to form a variable capacitor.

[0008] The number of the grooves is greater than or equal to 2.

[0009] The number of the anode electrodes 7 is equal to the number of the grooves minus one.

[0010] The number of the P-type implantation regions 8 is equal to the number of the grooves minus one.

[0011] The groove is in the shape of a circle, a rectangle or a polygon with 4 or more sides.

[0012] The grooves are respectively concentric or parallel to each other depending on their shapes.

[0013] The doping material of the P-type region 8 is Mg, and the doping concentration is 1×10 14 -1×10 20 cm -3 .

[0014] The bottom two layers of the metal material of the cathode electrode 6 are Ti / Al, Ta / Al, or Mo / Al; or there are a third layer or more of metal materials, the third layer or more of metal materials are Ni / Au, Ti / Au, Pt / Au, Mo / Au, or TiN, and the total thickness is 100-500nm;

[0015] The bottom metal layer of the anode electrode 7 is Ni, Ti, W or Mo, and the second layer and above can be Al, Au or TiN, with a total thickness of 100-1000 nm.

[0016] A passivation layer 5 is disposed above the barrier layer 4 between the cathode electrode 6 and the anode electrode 7;

[0017] The material of the passivation layer 5 is any one or more of Si3N4, SiO2, Al2O3 or HfO2.

[0018] The material of the composite channel layer 3 and the barrier layer 4 is a group III nitride semiconductor, including one of GaN, AlN, InN or a compound composed of any two or more of them in any ratio, with a thickness of 30-300nm;

[0019] The composite channel layer (3) comprises a channel layer (32) and an insertion layer (31).

[0020] The substrate layer 1 is made of one of silicon, silicon carbide, sapphire and diamond, and has a thickness of 100-1500 μm.

[0021] The composite buffer layer 2 is provided with a nucleation layer 21, a transition layer 22 and a buffer layer 23 in sequence from bottom to top;

[0022] The nucleation layer 21 is made of AlN and has a thickness of 50-300 nm;

[0023] The transition layer 22 is made of AlGaN with a gradient Al content, where the Al content changes from 0.75 to 0.15 and the thickness is 100nm-1μm;

[0024] The buffer layer 23 is made of GaN or AlGaN, and has a thickness of 100 nm-10 μm.

[0025] A method for preparing a lateral gallium nitride-based varactor comprises the following steps:

[0026] Step S1, selecting a substrate layer and cleaning it;

[0027] Step S2, growing an epitaxial wafer: sequentially growing a nucleation layer 21, a transition layer 22, a buffer layer 23, a composite channel layer 3 and a barrier layer 4 on the substrate layer 1 cleaned in step S1 to prepare an epitaxial wafer;

[0028] Step S3, preparing a P-type implantation region 8: performing photolithography on the upper surface of the barrier layer 4 of the epitaxial wafer prepared in step S2 to form a plurality of P-type implantation regions 8, injecting Mg ions into the plurality of P-type implantation regions 8, wherein the depth of the implanted Mg ions exceeds the position of the two-dimensional electron gas between the composite channel layer 3 and the barrier layer 4, and activating the P-type implantation region 8 by high temperature annealing or low energy electron beam irradiation (LEEBI);

[0029] Step S4, etching grooves: a mask is made by photolithography on the non-etched area on the upper surface of the barrier layer 4 prepared in step S3, and then the barrier layer 4 is etched to the upper middle part of the composite channel layer 3 to obtain a plurality of adjacent grooves;

[0030] Step S5, preparing a cathode electrode: growing the metal of the cathode electrode 6 in the groove obtained in step S4, and then performing high temperature annealing on the metal of the cathode electrode 6 to form an ohmic contact;

[0031] Step S6, preparing the anode electrode: growing the metal of the anode electrode 7 in other grooves based on step S5;

[0032] Step S7, preparing a passivation layer: on the basis of step S6, a passivation layer 5 is deposited on the barrier layer 4 between the cathode 6 and the plurality of anode electrodes 7 and on the barrier layer 4 between the plurality of anode electrodes 7 by using a plasma chemical vapor deposition (PECVD) or plasma atomic layer deposition (PEALD) method.

[0033] Compared with the prior art, the beneficial effects of the present invention are:

[0034] 1. The present invention utilizes a P-type injection region to realize the capacitance variation of a gallium nitride PN junction diode, and utilizes a coil-shaped structure to realize parallel connection of multiple PN junction diodes, thereby achieving a larger capacitance variation range on the same structure.

[0035] 2. The present invention utilizes the two-dimensional electron gas of gallium nitride material, whose high electron mobility characteristics help to achieve a high current density of the diode. Compared with other materials, it achieves more space charge capacitance after the diode is pressurized.

[0036] 3. The present invention utilizes gallium nitride as a base to realize a lateral varactor diode, avoiding the defects caused by the vertical gallium nitride diode structure material, and is compatible with other currently mainstream gallium nitride radio frequency device processes.

[0037] In summary, compared with the prior art, the present invention introduces a lateral structure into the GaN-based varactor, which can realize parallel connection of multiple varactor diodes on the lateral gallium nitride-based heterojunction structure, and has the characteristics of being able to improve the capacitance range of the variable capacitor and being easy to prepare. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic structural diagram of a lateral gallium nitride-based varactor according to Example 1 of the present invention.

[0039] Figure 2 It is a top view of the structure of the lateral gallium nitride-based varactor according to Example 1 of the present invention.

[0040] Figure 3It is a schematic structural diagram of a lateral gallium nitride-based varactor according to embodiment 3 of the present invention.

[0041] Figure 4 It is a top view of the structure of a lateral gallium nitride-based varactor according to Example 3 of the present invention.

[0042] Figure 5 It is a top view of the structure of a lateral gallium nitride-based varactor according to embodiment 5 of the present invention.

[0043] Figure 6 It is a flow chart of the method for preparing a lateral gallium nitride-based varactor according to Example 2 of the present invention.

[0044] Among them: 1. substrate layer; 2. composite buffer layer; 21. nucleation layer; 22. transition layer; 23. buffer layer; 3. composite channel layer; 31. channel layer; 32. insertion layer; 4. barrier layer; 5. passivation layer; 6. cathode; 7. anode; 8. P-type injection region. DETAILED DESCRIPTION

[0045] The present invention will be described in detail below in conjunction with the accompanying drawings.

[0046] Example 1

[0047] The present invention provides a lateral gallium nitride-based variable capacitor structure as follows Figure 1 As shown, the top view is Figure 2 As shown, from bottom to top, it includes a substrate layer 1, a composite buffer layer 2, a composite channel layer 3 and a barrier layer 4; a heterojunction is formed between the composite channel layer 3 and the barrier layer 4, and the heterojunction polarization forms a two-dimensional electron gas (2DEG) on one side of the composite channel layer 3; 20 grooves are arranged on the barrier layer 4 and part of the composite channel layer 3, and the bottom ends of the grooves penetrate the barrier layer 4 and the two-dimensional electron gas to the upper and middle parts of the composite channel layer 3; cathode electrodes 6 are arranged in 13 grooves, anode electrodes 7 are arranged in 7 grooves, and 7 P-type regions 8 are arranged on the side close to the anode electrodes in the grooves where the anode electrodes 7 are arranged; the P-type regions 8 respectively form PN junctions with the barrier layer 4 and part of the composite channel layer 3 close to the cathode electrode 6, and the PN junction and the cathode electrode 6 are respectively connected to the anode electrode 7 to form a PN junction diode, and the capacitance of the PN junction diode changes when pressure is applied to form a variable capacitor.

[0048] The groove is in the shape of a rectangle, and the other grooves are closed rectangular coils.

[0049] The grooves are parallel to each other.

[0050] The doping material of the P-type region 8 is Mg, and the doping concentration is 5×10 19 cm -3 .

[0051] The bottom two layers of the metal material of the cathode electrode 6 are Ti / Al; the third layer and above are Ni / Au, with a total thickness of 250 nm.

[0052] The bottom layer of the metal material of the anode electrode 7 is Ni, the second layer is Au, and the total thickness is 300 nm.

[0053] The material of the passivation layer 5 is Si3N4, and the thickness is 200 nm.

[0054] The composite channel layer 3 is made of GaN with a thickness of 500 nm, and the barrier layer 4 is made of AlGaN with a thickness of 20 nm.

[0055] The bottom layer 1 is made of high-resistance silicon and has a thickness of 625 μm.

[0056] The thickness of the nucleation layer 21 is 200 nm.

[0057] The transition layer 22 has a thickness of 700 nm.

[0058] The buffer layer 23 is made of GaN and has a thickness of 1 μm.

[0059] Example 2

[0060] This embodiment provides a method for preparing a lateral GaN-based varactor. Figure 6 As shown, the specific implementation steps are as follows:

[0061] Step S1, selecting a substrate layer and cleaning it: selecting a substrate layer 1, passing hydrogen at 900° C., and cleaning the surface of the substrate layer 1 to remove pollutants on the surface of the substrate layer 1. In this embodiment, the substrate layer material is 400 μm silicon;

[0062] Step S2, growing epitaxial wafer:

[0063] Using a metal organic chemical vapor deposition (MOCVD) method, at 1000°C, with TMGa and NH3 as reaction gases, a 100nm AlN nucleation layer 21, a 1μm Al0.3Ga0.7N transition layer 22, a 300nm GaN buffer layer 23, a 50nm GaN composite channel layer 3 and a 10nm AlGaN barrier layer 4 are sequentially epitaxially grown on the substrate layer to form an epitaxial wafer;

[0064] Step S3, preparing a P-type implantation region 8:

[0065] On the basis of the epitaxial wafer, two P-type implantation regions on the surface of the barrier layer 4 are exposed by photolithography, and Mg ions are implanted into the two P-type implantation regions. The implantation ion concentration is 1x1017cm-3, and the implantation depth of the P-type implantation region is 30nm. After the implantation, a high-temperature annealing process is used to activate the ions in a N2 atmosphere at a temperature of 850°C, thereby obtaining a P-type implantation region 8;

[0066] Step S4, etching grooves:

[0067] After the etching area is exposed by photolithography on the barrier layer 4 on the basis of step S3, the barrier layer 4 is etched by reactive ion etching equipment and technology (RIE) to the upper middle part of the composite channel layer 3 to obtain three adjacent grooves with an etching depth of 30 nm;

[0068] Step S5, preparing the cathode electrode:

[0069] Based on step S4, a photolithography process is used to make a photoresist mask to expose the central groove cathode electrode area where the cathode metal is to be deposited; then 30nm / 100nm of metal Ti / Al is grown in the cathode electrode area by electron beam evaporation, wherein Ti is the first layer of metal, directly contacting the bottom of the groove, and then rapid annealing is performed under N2 at a temperature of 850°C for 30s to alloy and form an ohmic contact;

[0070] Step S6: preparing the anode electrode:

[0071] Based on step S5, a photolithography process is used to make a photoresist mask to expose two anode electrode areas of the groove where the anode metal is to be deposited; then two anode electrodes are prepared by electron beam evaporation technology, and 45nm / 200nm / 200nm of metal Ni / Au / Ni are evaporated in sequence. After the evaporation is completed, the metal is annealed by thermal annealing at a temperature of 425°C for 10 minutes to form a Schottky contact;

[0072] Step S7, preparing a passivation layer: using plasma enhanced chemical vapor deposition (PECVD) in an atmosphere of 300° C., a layer of Si 3 N 4 film with a thickness of 150 nm is deposited on the barrier layer 4 between the cathode 6 and the two anode electrodes 7 and on the barrier layer 4 between the two anode electrodes 7.

[0073] Example 3

[0074] The present invention provides a lateral gallium nitride-based variable capacitor structure as follows Figure 3 As shown, the top view is Figure 4As shown, from bottom to top, it includes a substrate layer 1, a composite buffer layer 2 (nucleation layer 21, transition layer 22 and buffer layer 23), a composite channel layer 3 (channel layer 32 and insertion layer 31) and a barrier layer 4. A two-dimensional electron gas with high electron mobility is formed in the composite channel layer 3 near the interface between the composite channel layer 3 and the barrier layer 4. A plurality of grooves are arranged between the barrier layer 4 and the composite channel layer 3. The bottom of the groove penetrates the barrier layer 4 to the middle and upper part of the composite channel layer 3. The shape of the central groove is circular, and the shape of the other grooves is a circular ring with the center as a concentric circle. A cathode electrode 6 is arranged in the concentric grooves of all the grooves, and the contact of the cathode electrode is an ohmic contact. A plurality of anode electrodes 7 are arranged in the other grooves, and the contact of the anode electrode is a Schottky contact. A plurality of P-type injection regions 8 are arranged around the grooves near the cathode electrode, and the injection depth of the P-type injection region 8 is greater than or equal to the groove depth.

[0075] The difference from the second embodiment is that the substrate layer 1 of the present embodiment is made of sapphire with a thickness of 300 μm.

[0076] The difference from Example 2 is that the epitaxial wafer is grown by MOCVD method, the temperature is 1000° C., and the material of the grown barrier layer 4 is In0.17Al0.83N with a thickness of 15 nm.

[0077] The difference from Example 2 is that two layers are distinguished in the composite channel layer 3, namely the channel layer 32 and the insertion layer 31. The epitaxial wafer is grown by MOCVD method at a temperature of 1000°C. The grown channel layer 32 is GaN with a thickness of 30nm, and the insertion layer 31 is AlN with a thickness of 0.5nm. The insertion layer 31 can increase the channel electron density and electron mobility, and improve the effect of the heterogeneous interface.

[0078] The difference from Example 2 is that plasma atomic layer deposition (PEALD) is used to grow the Al2O3 passivation layer 5 with a thickness of 150 nm.

[0079] Example 4

[0080] The present invention provides a method for preparing a lateral gallium nitride-based varactor, which is specifically implemented according to the following steps:

[0081] Step S1, selecting a substrate layer and cleaning it: selecting a substrate layer 1, passing hydrogen at 900° C., and cleaning the surface of the substrate layer 1 to remove pollutants on the surface of the substrate layer 1. In this embodiment, the substrate layer material is 400 μm silicon;

[0082] Step S2, growing epitaxial wafer:

[0083] Using MOCVD method, at a temperature of 1000° C., a 100nm AlN nucleation layer 21, a 1μm Al0.3Ga0.7N transition layer 22, a 200nm GaN buffer layer 23, a 30nm GaN channel layer 32, a 0.5nm AlN insertion layer 31 and a 15nm AlGaN barrier layer 4 are sequentially epitaxially grown on the substrate layer to form an epitaxial wafer;

[0084] Step S3, preparing a P-type implantation region 8:

[0085] On the basis of step S2, three P-type implantation regions 8 on the upper surface of the barrier layer 4 are exposed by photolithography, and Mg ions are implanted into the three P-type implantation regions 8, with an implantation concentration of 1×1016 cm-3 and an implantation depth of 45 nm. After the implantation, a high temperature annealing process is used to perform activation treatment in a N2 atmosphere at a temperature of 800° C.;

[0086] Step S4, etching grooves:

[0087] After a photolithography step is performed on the barrier layer 4 to expose the etching area based on step S3, the barrier layer 4 is etched using reactive ion etching equipment and technology (RIE) to the middle and upper part of the channel layer 32 to obtain four adjacent grooves with an etching depth of 300 nm.

[0088] Step S5, preparing the cathode electrode:

[0089] Based on step S4, a photolithography process is used to make a photoresist mask to expose the central groove cathode electrode area where the cathode metal is to be deposited; then 30nm / 100nm of metal Ti / Al is grown in the cathode electrode area by electron beam evaporation, wherein Ti is the first layer of metal, directly contacting the bottom of the groove, and then rapid annealing is performed under N2 at a temperature of 850°C for 30s to alloy and form an ohmic contact;

[0090] Step S6: preparing the anode electrode:

[0091] On the basis of step S5, a photolithography process is used to make a photoresist mask to expose two grooved anode electrode areas where the anode metal is to be deposited; then, two anode electrodes are prepared by electron beam evaporation technology, and 45nm / 200nm / 200nm of metal Ni / Au / Ni are evaporated in sequence. After the evaporation is completed, the device is annealed in an annealing furnace at a temperature of 400°C for 10 minutes to form a Schottky contact.

[0092] Step S7, preparing a passivation layer: using a plasma atomic layer deposition (PEALD) process, a layer of Al2O3 film with a thickness of 150 nm is deposited on the barrier layer 4 between the cathode 6 and the two anode electrodes 7 and on the barrier layer 4 between the two anode electrodes 7.

[0093] Example 5

[0094] A top view of a lateral gallium nitride-based varactor structure of the present invention is shown in FIG. Figure 5 As shown. This embodiment includes a substrate layer 1, a composite buffer layer 2, a composite channel layer 3 and a barrier layer 4 from bottom to top; a heterojunction is formed between the composite channel layer 3 and the barrier layer 4, and the heterojunction polarization forms a two-dimensional electron gas (2DEG) on one side of the composite channel layer 3; 5 grooves are arranged on the barrier layer 4 and part of the composite channel layer 3, and the bottom of the groove penetrates the barrier layer 4 and the two-dimensional electron gas to the middle and upper part of the composite channel layer 3; the shape of the groove is a rectangular strip; a cathode electrode 6 is arranged in part of the groove, and an anode electrode 7 is arranged in the remaining grooves, and a P-type region 8 is arranged on the side close to the anode electrode in the groove where the anode electrode 7 is arranged; the P-type region respectively forms a PN junction with the barrier layer 4 and part of the channel layer 3 on the side close to the cathode electrode 6, and the PN junction and the cathode electrode 6 are respectively connected to the anode electrode 7 to form a PN junction diode, and the capacitance of the PN junction diode changes when pressure is applied to form a variable capacitor.

[0095] In this embodiment, the substrate layer 1 is made of silicon nitride with a thickness of 500μm; the nucleation layer 21 is made of AlN with a thickness of 200nm; the transition layer 22 is made of AlGaN with a thickness of 500nm; the buffer layer 23 is made of GaN with a thickness of 1000nm; the composite channel layer 3 is made of GaN with a thickness of 300nm; the barrier layer 4 is made of AlGaN with a thickness of 20nm, the passivation layer 6 is made of SiO2 with a thickness of 150nm; the cathode 6 is made of Ta / Al / Ni / Au (20nm / 120nm / 40nm / 50nm); and the anodes 7 and 8 are made of Ti / Au (50nm / 280nm).

[0096] A method for preparing a lateral gallium nitride-based varactor comprises the following steps:

[0097] Step S1, selecting and cleaning the substrate layer: selecting a silicon carbide substrate layer 1 with a thickness of 500 μm, and cleaning the surface of the substrate layer 1 under the condition of 1000° C. with hydrogen to remove contaminants on the surface of the substrate layer 1;

[0098] Step S2, growing epitaxial wafer:

[0099] Using MOCVD method at 600°C, a 200nm AlN nucleation layer 21 is grown on the surface of the substrate layer 1;

[0100] The temperature is raised to 1000° C., and an Al0.75Ga0.25N transition layer 22 with a thickness of 500 nm and a GaN buffer layer 23 with a thickness of 1000 nm are sequentially grown on the nucleation layer by a MOCVD method;

[0101] Using the MOCVD method, the temperature is set to 1000° C., and a GaN composite channel layer 3 with a thickness of 300 nm is grown on the buffer layer;

[0102] Using the MOCVD method, the temperature is set to 1000° C., and an AlGaN barrier layer 4 with a thickness of 20 nm is epitaxially grown on the composite channel layer 3;

[0103] Step S3, preparing P-type injection area 8: Based on the epitaxial wafer, four P-type injection areas 8 on the upper surface of the barrier layer 4 are exposed by photolithography steps, and Mg ions are injected into the four P-type injection areas 8. The injection ion concentration is 1x1020cm-3 and the injection depth is 100nm. After the injection, a high-temperature annealing process is used to activate the ions in a N2 atmosphere at a temperature of 850°C.

[0104] Step S4, etching grooves: Based on step 3, after a photolithography step is performed on the barrier layer 4 to expose the etching area, the barrier layer 4 is etched using reactive ion etching equipment and technology (RIE) to the upper and middle parts of the composite channel layer 3 to obtain 5 adjacent grooves with an etching depth of 300nm.

[0105] Step S5, preparing the cathode electrode:

[0106] Using the coating, pre-baking and exposure process, the photoresist in the central groove etched in step 4 is removed, and the area where the cathode electrode 6 is to be formed is exposed by development;

[0107] Electron beam evaporation is used to grow multiple layers of metal Ta / Al / Ni / Au in the cathode electrode 6 region, namely, from bottom to top: 20 nm thick Ta, 120 nm thick Al, 40 nm thick Ni, 50 nm thick Au;

[0108] The prepared cathode electrode 6 metal is placed in an annealing furnace and subjected to rapid thermal annealing for 30 seconds in a N2 atmosphere at 830°C to form an ohmic contact.

[0109] Step S6: preparing the anode electrode:

[0110] Using the coating, pre-baking and exposure processes, the photoresist in the grooves other than the center etched in step S4 is removed, and the areas where the anode electrodes are to be made are exposed by development;

[0111] Electron beam evaporation is used to grow multiple layers of metal Ti / Al / Mo / Au in the cathode electrode area to form a cathode electrode with a thickness of 30nm / 100nm / 30nm / 100nm, where Ti is the bottom metal directly contacting the bottom of the groove;

[0112] The deposited anode metal is placed in an annealing furnace and thermally annealed in a N2 atmosphere at 450°C for 10 minutes to form a Schottky contact.

[0113] Step S7, prepare a passivation layer: use plasma enhanced chemical vapor deposition (PECVD) in an atmosphere of 300°C to deposit a SiO2 film with a thickness of 150nm on the barrier layer 4 between the cathode electrode 6 and several anode electrodes 7 and on the barrier layer 4 between the four anode electrodes 7 and the P-type injection region 8.

[0114] The above contents are further detailed descriptions of the present invention in combination with specific embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A lateral gallium nitride-based varactor structure, characterized in that: The invention comprises, from bottom to top, a substrate layer (1), a composite buffer layer (2), a composite channel layer (3) and a barrier layer (4); a heterojunction is formed between the composite channel layer (3) and the barrier layer (4); the heterojunction polarization forms a two-dimensional electron gas on one side of the composite channel layer (3); a plurality of grooves are arranged on the barrier layer (4) and part of the composite channel layer (3); the bottom ends of the grooves penetrate the barrier layer (4) and the two-dimensional electron gas to the middle and upper part of the composite channel layer (3); a cathode electrode (6) is arranged in part of the grooves, an anode electrode (7) is arranged in the remaining grooves, and a P-type injection region (8) is arranged on the side close to the anode electrode in the groove where the anode electrode (7) is arranged; the P-type injection region (8) respectively forms a PN junction with the barrier layer (4) and part of the composite channel layer (3) on the side close to the cathode electrode (6); the PN junction and the cathode electrode (6) are respectively connected to the anode electrode (7) to form a PN junction diode; the capacitance of the PN junction diode changes when voltage is applied to form a variable capacitor.

2. The lateral gallium nitride-based varactor structure according to claim 1, characterized in that: The number of the grooves is greater than or equal to 2; The number of the anode electrodes (7) is equal to the number of grooves minus 1; The number of the P-type implantation regions (8) is equal to the number of the grooves minus 1.

3. The lateral gallium nitride-based varactor structure according to claim 1, characterized in that: The groove is in the shape of a circle, a rectangle or a polygon with 4 or more sides; The grooves are respectively concentric or parallel to each other depending on their shapes.

4. The lateral gallium nitride-based varactor according to claim 1, characterized in that: The doping material of the P-type injection region (8) is Mg, and the doping concentration is 1×1014-1×1020 cm-3.

5. The lateral gallium nitride-based varactor according to claim 1, characterized in that: The bottom two layers of the metal material of the cathode electrode (6) are Ti / Al, Ta / Al, or Mo / Al; or there are a third layer or more of metal materials, and the third layer or more of metal materials are Ni / Au, Ti / Au, Pt / Au, Mo / Au, or TiN, with a total thickness of 100-500nm; The bottom layer of the metal material of the anode electrode (7) is Ni, Ti, W or Mo, and the second layer and above can be Al, Au or TiN, with a total thickness of 100-1000 nm.

6. The lateral gallium nitride-based varactor according to claim 1, characterized in that: A passivation layer (5) is provided above the barrier layer (4) between the cathode electrode (6) and the anode electrode (7); The material of the passivation layer (5) is any one or more of Si3N4, SiO2, Al2O3 or HfO2.

7. The lateral gallium nitride-based varactor according to claim 1, characterized in that: The materials of the composite channel layer (3) and the barrier layer (4) are group III nitride semiconductors, including one of GaN, AlN, and InN, or a compound composed of any two or more of them in any ratio, with a thickness of 30-300 nm; The composite channel layer (3) comprises a channel layer (32) and an insertion layer (31); The substrate layer (1) is made of one of silicon, silicon carbide, sapphire and diamond, and has a thickness of 100-1500 μm.

8. The lateral gallium nitride-based varactor according to claim 1, characterized in that: The composite buffer layer (2) is provided with a nucleation layer (21), a transition layer (22) and a buffer layer (23) in sequence from bottom to top; The nucleation layer (21) is made of AlN and has a thickness of 50-300 nm; The transition layer (22) is made of AlGaN with a gradient Al composition, wherein the Al composition gradiently changes from 0.75 to 0.15 and the thickness is 100nm-1μm; The buffer layer (23) is made of GaN or AlGaN and has a thickness of 100 nm-10 μm.

9. A method for preparing a lateral gallium nitride-based varactor, characterized in that: The specific steps include: Step S1, selecting a substrate layer and cleaning it; Step S2, growing an epitaxial wafer: sequentially growing a nucleation layer (21), a transition layer (22), a buffer layer (23), a composite channel layer (3) and a barrier layer (4) on the substrate layer (1) cleaned in step S1 to prepare an epitaxial wafer; Step S3, preparing a P-type implantation region (8): performing photolithography on the upper surface of the barrier layer (4) of the epitaxial wafer prepared in step S2 to form a plurality of P-type implantation regions (8), implanting Mg ions into the plurality of P-type implantation regions (8), wherein the depth of the implanted Mg ions exceeds the position of the two-dimensional electron gas between the composite channel layer 3 and the barrier layer 4, and activating the P-type implantation region by high temperature annealing or low energy electron beam irradiation (LEEBI); Step S4, etching grooves: a mask is made by photolithography on the non-etched area on the upper surface of the barrier layer (4) prepared in step S3, and then the barrier layer (4) is etched to the middle and upper part of the composite channel layer (3) to obtain a plurality of adjacent grooves; Step S5, preparing a cathode electrode: growing the metal of the cathode electrode (6) in the groove obtained in step S4, and then performing high temperature annealing on the metal of the cathode electrode (6) to form an ohmic contact; Step S6, preparing the anode electrode: growing the metal of the anode electrode 7 in other grooves based on step S5; Step S7, preparing a passivation layer: on the basis of step S6, a passivation layer (5) is deposited on the barrier layer (4) between the cathode (6) and the plurality of anode electrodes (7) and on the barrier layer (4) between the plurality of anode electrodes (7) by using a plasma chemical vapor deposition (PECVD) or plasma atomic layer deposition (PEALD) method.

Citation Information

Patent Citations

  • Semiconductor heterojunction varactor device with lateral structure

    CN108365019A

  • Variable capacitance diode and manufacturing method thereof

    JP2007273886A

  • Varactor diode with doped voltage blocking layer

    US20100059850A1

  • Semiconductor device and manufacturing method thereof

    US20120056196A1