Solar cell, preparation method thereof and photovoltaic module
By using a combination of a silicon substrate, a multi-layer doped structure and an intrinsic amorphous silicon layer in solar cells, and combining a transparent conductive oxide film, the problems of high composite current density and low conversion efficiency of existing hybrid solar cells are solved. Achieve more efficient energy conversion and performance improvements.
Patent Information
- Application Number
- CN202411022448.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing hybrid solar cells have high composite current density and low conversion efficiency, which cannot meet the ever-changing needs of users.
Using a combined structure of a silicon substrate, a tunneling layer, a light doped layer, a first doped layer and a heavily doped layer, combined with an intrinsic amorphous silicon layer and a transparent conductive oxide film, it is activated by annealing and passivation layer. A hybrid solar cell structure with low contact resistance is formed to reduce parasitic absorption and optical loss.
It effectively reduces the composite current density of solar cells, improves conversion efficiency, reduces optical loss, and improves the performance stability of the battery.
Smart Images

Figure CN118969861A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field related to solar cells, and in particular to a solar cell and a preparation method thereof, and a photovoltaic module. Background Art
[0002] With the continuous advancement of photovoltaic technology, researchers are actively exploring and developing various new solar cell technologies to improve efficiency and reduce costs. Crystalline silicon solar cells are still the most mainstream type of solar cells on the market due to their high efficiency and good stability. However, each cell technology has its limitations, so combining different types of cells to prepare hybrid cells is an effective way.
[0003] Hybrid solar cells are created by combining different types of solar cell technologies to create new types of photovoltaic devices, aiming to combine the advantages of various cell technologies to improve overall performance and reduce costs. This approach allows researchers to explore new photovoltaic solutions to address the limitations that a single technology may face. Challenges of hybrid solar cells include compatibility of manufacturing processes, improvement of material stability, cost control, and long-term stability of cell performance. Researchers are constantly exploring new materials, designs, and manufacturing techniques to achieve these goals. As technology advances, hybrid solar cells are expected to play an important role in improving energy conversion efficiency and reducing costs.
[0004] The current hybrid batteries have high composite current density and low conversion efficiency, which cannot meet the ever-changing needs of users. Summary of the invention
[0005] The object of the present invention is to provide a solar cell and a preparation method thereof, and a photovoltaic module, so as to reduce the composite current density of the cell and improve the conversion efficiency of the cell.
[0006] In order to solve the above technical problems, the present invention provides a solar cell and a preparation method thereof, and a photovoltaic module.
[0007] The solar cell of the present invention comprises a silicon substrate, a first surface and a second surface;
[0008] The first surface and the second surface are arranged opposite to each other;
[0009] A tunneling layer, a lightly doped layer, a first doped layer and a heavily doped layer are sequentially provided between the silicon substrate and the first surface starting from the silicon substrate, wherein the first doped layer is doped with at least one element of oxygen or carbon;
[0010] An intrinsic amorphous silicon layer is disposed between the silicon substrate and the second surface.
[0011] Furthermore, the first doped layer is an oxygen-doped polysilicon layer, a carbon-doped polysilicon layer, or a polysilicon layer doped with both oxygen and carbon.
[0012] Furthermore, the thickness of the first doping layer is in the range of 50-100 nanometers.
[0013] Furthermore, the heavily doped layer has a thickness ranging from 30 to 60 nanometers.
[0014] Furthermore, the thickness of the lightly doped layer is in the range of 5-10 nanometers.
[0015] Furthermore, the first surface is a light-facing surface of the solar cell, and the second surface is a light-backed surface of the solar cell.
[0016] Furthermore, a passivation layer and a first electrode are disposed on the heavily doped layer, the first electrode is connected to the heavily doped layer, and the passivation layer covers the heavily doped layer and exposes the first electrode.
[0017] Furthermore, the passivation layer is silicon nitride or aluminum oxide.
[0018] Furthermore, the intrinsic amorphous silicon layer is intrinsic amorphous silicon containing oxygen, intrinsic amorphous silicon containing carbon, or intrinsic amorphous silicon containing nitrogen.
[0019] Furthermore, a second doping layer is disposed between the intrinsic amorphous silicon layer and the second surface, and the doping type of the second doping layer is opposite to that of the silicon substrate.
[0020] Furthermore, the second doped layer is a doped amorphous silicon layer or a doped microcrystalline silicon layer.
[0021] Furthermore, the silicon substrate, the lightly doped layer and the heavily doped layer are all N-type doped.
[0022] Furthermore, a transparent conductive oxide film is disposed between the intrinsic amorphous silicon layer and the second surface, a second electrode is disposed on the transparent conductive oxide film, and the transparent conductive oxide film is connected to the second electrode.
[0023] Furthermore, it also includes a reflection enhancement layer, which covers the transparent conductive oxide film and exposes the second electrode.
[0024] The present invention also provides a method for preparing a solar cell, comprising:
[0025] providing a silicon substrate;
[0026] Forming a tunneling layer, a lightly doped layer, a first doped layer and a heavily doped layer in sequence from one surface of the silicon substrate, and doping the first doped layer with at least one element of oxygen or carbon;
[0027] Performing annealing treatment on the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer;
[0028] An intrinsic amorphous silicon layer is formed on the other surface of the silicon substrate.
[0029] Furthermore, before forming the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer, the silicon substrate is textured and first cleaned.
[0030] Furthermore, after the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer are annealed, a passivation layer is formed on the heavily doped layer, and the passivation layer is activated.
[0031] Furthermore, the other surface of the silicon substrate is subjected to a second cleaning, then polishing, and then a third cleaning to form the intrinsic amorphous silicon layer; a second doped layer is formed on the intrinsic amorphous silicon layer, a transparent conductive oxide film is formed on the second doped layer, a first electrode is formed on the heavily doped layer, and a second electrode is formed on the transparent conductive oxide film.
[0032] Furthermore, a reflection enhancement layer is formed on the transparent conductive oxide film and the second electrode is exposed.
[0033] The present invention further provides a photovoltaic assembly, comprising a plurality of solar cells as described in any one of the above technical solutions connected in series and / or in parallel.
[0034] Compared with the prior art, the present invention has at least the following beneficial effects:
[0035] The present application combines a passivated contact solar cell structure with a tunneling layer with a heterojunction solar cell structure to form a hybrid solar cell, wherein the three-layer doping structure of the lightly doped layer, the first doped layer and the heavily doped layer cooperate with each other, and the heavily doped layer is used as the contact area with the electrode, which can reduce the contact resistance. Due to the existence of the first doped layer, there is no need to set a thicker heavily doped layer while ensuring passivation, so that parasitic absorption will not be greatly increased, and the lightly doped layer can reduce the damage of the first doped layer to the tunneling layer, and the lightly doped layer also further reduces the parasitic absorption. The three work together to reduce the optical loss of the solar cell, which is beneficial to reducing the composite current density of the solar cell and improving the conversion efficiency of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 A schematic structural diagram of an embodiment of a solar cell of the present invention;
[0037] Figure 2The present invention is a flow chart of an embodiment of a method for preparing a solar cell.
[0038] 1. Silicon substrate; 2. Tunneling layer; 3. Lightly doped layer; 4. First doped layer; 5. Heavily doped layer; 6. Passivation layer; 7. Intrinsic amorphous silicon layer; 8. Second doped layer; 9. Transparent conductive oxide film; 10. First electrode; 11. Reflection enhancement layer; 12. Second electrode. DETAILED DESCRIPTION
[0039] A solar cell and a method for preparing the same, and a photovoltaic module of the present invention will be described below in conjunction with schematic diagrams, wherein preferred embodiments of the present invention are shown. It should be understood that those skilled in the art may modify the present invention described herein while still achieving the advantageous effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art, and not as a limitation of the present invention.
[0040] The serial numbers of the components herein, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in this application, unless otherwise specified, include direct and indirect connections (couplings). In the description of the present invention, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc. are based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to the present invention.
[0041] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0042] The present invention is described in more detail in the following paragraphs by way of example with reference to the accompanying drawings. The advantages and features of the present invention will become more apparent from the following description and claims. It should be noted that the drawings are in very simplified form and in non-precise proportions, and are only used to facilitate and clearly assist in illustrating the purpose of the embodiments of the present invention.
[0043] The following is attached to the instruction manual Figure 1 , the solar cell according to the first embodiment of the present invention is introduced.
[0044] In one embodiment, if Figure 1 As shown, the solar cell comprises a silicon substrate 1, a first surface and a second surface, wherein the first surface and the second surface are arranged opposite to each other.
[0045] A tunneling layer 2, a lightly doped layer 3, a first doped layer 4 and a heavily doped layer 5 are sequentially arranged between the silicon substrate 1 and the first surface, wherein the first doped layer is doped with at least one element of oxygen or carbon, and the first doped layer 4 is used to reduce parasitic absorption while ensuring passivation. An intrinsic amorphous silicon ( i -μ- Si ) layer 7.
[0046] The solar cell of the present application is formed by combining a passivation contact solar cell structure with a tunneling layer 2 and a heterojunction solar cell structure, wherein the first doping layer 4 is doped with at least one element of oxygen or carbon to reduce parasitic absorption while ensuring passivation. The three-layer doping structure of the lightly doped layer 3, the first doping layer 4 and the heavily doped layer 5 cooperate with each other, and the heavily doped layer 5 is used as the contact area with the electrode to reduce the contact resistance. Due to the existence of the first doping layer 4, there is no need to set a thicker heavily doped layer 5 while ensuring passivation, so that the parasitic absorption will not be greatly increased, and the lightly doped layer 3 can reduce the damage of the first doping layer 4 to the tunneling layer 2, and the lightly doped layer 3 also further reduces the parasitic absorption. The three work together to reduce the optical loss of the solar cell, which is beneficial to reducing the composite current density of the solar cell and improving the conversion efficiency of the solar cell.
[0047] Exemplarily, the doping type of the silicon substrate 1 can be N-type or P-type. When the silicon substrate 1 is N-type doped, Group V elements such as phosphorus or arsenic are used as doping elements. When the silicon substrate 1 is P-type doped, Group III elements such as boron or gallium are used as doping elements.
[0048] Specifically, the lightly doped layer 3 refers to a doped polysilicon layer manufactured by a lightly doping process, and the heavily doped layer 5 refers to a doped polysilicon layer manufactured by a heavily doping process.
[0049] In one embodiment, the first doped layer 4 is an oxygen-doped polysilicon (poly-Si) layer. In other embodiments, it can also be a carbon-doped polysilicon layer, or a polysilicon layer doped with both oxygen and carbon. Among them, doping with carbon and / or oxygen elements can reduce the parasitic absorption of the polysilicon layer. Although the introduction of carbon and / or oxygen elements will introduce damage to the tunneling layer 2, the provision of a lightly doped layer 3 can reduce the damage to the tunneling layer 2.
[0050] In one embodiment, preferably, the thickness of the first doping layer 4 is in the range of 50-100 nanometers. For example, the thickness of the first doping layer 4 can be set to 60 millimeters. In other embodiments, the thickness of the first doping layer 4 can also be set to 80 millimeters. Of course, other thicknesses can also be used as needed.
[0051] In one embodiment, preferably, the thickness of the heavily doped layer 5 is in the range of 30-60 nanometers. For example, the thickness of the heavily doped layer 5 can be set to 30 millimeters. In other embodiments, the thickness of the heavily doped layer 5 can also be set to 40 millimeters. Of course, other thicknesses can also be used as needed. It should be noted that the thinner the heavily doped layer 5, the lower the parasitic absorption, so the thinner the heavily doped layer 5 is, the better it is while ensuring the contact resistance.
[0052] In one embodiment, preferably, the thickness of the lightly doped layer 3 is in the range of 5-10 nanometers. For example, the thickness of the lightly doped layer 3 can be set to 5 millimeters. In other embodiments, the thickness of the lightly doped layer 3 can also be set to 8 millimeters. Of course, other thicknesses can also be used as needed.
[0053] In one embodiment, the first surface is the light-facing surface of the solar cell, and the second surface is the backlight surface of the solar cell. In other embodiments, the first surface may also be the backlight surface of the solar cell, and the second surface is the light-facing surface of the solar cell.
[0054] In one embodiment, a passivation layer 6 and a first electrode 10 are provided on the heavily doped layer 5, the first electrode 10 is connected to the heavily doped layer 5, and the passivation layer 6 covers the heavily doped layer 5 and exposes the first electrode 10. The outer surface of the passivation layer 6 constitutes the first surface. The provision of the passivation layer 6 can reduce surface defects of the solar cell, increase the carrier lifetime, and prevent photocorrosion. Preferably, the passivation layer 6 is silicon nitride. In other embodiments, the passivation layer 6 can also be aluminum oxide.
[0055] The first electrode 10 may be a metal grid line, such as a silver-containing grid line or a copper-containing grid line.
[0056] In one embodiment, the intrinsic amorphous silicon layer 7 can play a passivation role in the solar cell. Specifically, the intrinsic amorphous silicon layer 7 can be intrinsic amorphous silicon containing oxygen. In other embodiments, the intrinsic amorphous silicon layer 7 can also be intrinsic amorphous silicon containing carbon or intrinsic amorphous silicon containing nitrogen.
[0057] In one embodiment, a second doped layer 8 is further disposed between the intrinsic amorphous silicon layer 7 and the second surface, and the second doped layer 8 is a doped amorphous silicon layer or a doped microcrystalline silicon layer.
[0058] In one embodiment, the doping type of the second doping layer 8 is opposite to that of the silicon substrate 1. For example, when the doping type of the silicon substrate 1 is N-type doping, the lightly doped layer 3, the first doping layer 4 and the heavily doped layer 5 are N-type doping, and the doping type of the second doping layer 8 is P-type doping, which can further improve the efficiency of the solar cell. When the doping type of the silicon substrate 1 is P-type doping, the lightly doped layer 3, the first doping layer 4 and the heavily doped layer 5 are P-type doping, and the doping type of the second doping layer 8 is N-type doping.
[0059] In another embodiment, when the doping type of the silicon substrate 1 is P-type doping, the lightly doped layer 3, the first doped layer 4 and the heavily doped layer 5 are still N-type doping, and the doping type of the second doped layer 8 is still P-type doping.
[0060] In one of the embodiments, a transparent conductive oxide film (TCO) 9 is further provided between the intrinsic amorphous silicon layer 7 and the second surface. The transparent conductive oxide film 9 has the dual functions of optical transparency and conductivity, plays a key role in the collection of effective carriers, can reduce the reflection of light, plays a good light trapping role, and is a good window layer material. For example, the transparent conductive oxide film 9 can be made of zinc oxide material, and in other embodiments, it can also be made of indium oxide or tin oxide material. Preferably, the thickness of the transparent conductive oxide film 9 ranges from 50 to 200 nanometers. For example, it can be 100 nanometers. In other embodiments, it can also be 80 nanometers. A second electrode 12 is provided on the transparent conductive oxide film 9, and the transparent conductive oxide film 9 is connected to the second electrode 12. The second electrode 12 can be a metal grid line, such as a silver-containing grid line or a copper-containing grid line.
[0061] In one embodiment, the solar cell further includes a reflection enhancement layer 11, and the outer side of the reflection enhancement layer 11 constitutes the second surface. Specifically, the reflection enhancement layer 11 can be made of a material with a high refractive index such as silicon or silicon dioxide to reduce the light loss reflected from the cell surface and improve the transmission and absorption of light, wherein the reflection enhancement layer 11 can be deposited on the transparent conductive oxide film 9 by evaporation. The reflection enhancement layer 11 covers the transparent conductive oxide film 9 and exposes the second electrode 12.
[0062] An embodiment of the second aspect of the present invention provides a method for preparing a solar cell.
[0063] In one embodiment, if Figure 2 As shown, the method for preparing the solar cell includes:
[0064] S100: providing a silicon substrate;
[0065] S200: forming a tunneling layer, a lightly doped layer, a first doped layer and a heavily doped layer in sequence from one surface of the silicon substrate, and doping the first doped layer with at least one element of oxygen or carbon;
[0066] S300: performing annealing treatment on the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer;
[0067] S400: forming an intrinsic amorphous silicon layer on the other surface of the silicon substrate.
[0068] In step S100, the silicon substrate is textured and first cleaned. The first cleaning may be a wet chemical cleaning method (RCA cleaning) or other cleaning methods.
[0069] The doping type of the silicon substrate can be N-type or P-type. When the silicon substrate 1 is N-type doped, a Group V element such as phosphorus or arsenic is used as a doping element. When the silicon substrate 1 is P-type doped, a Group III element such as boron or gallium is used as a doping element.
[0070] In step S200, a silicon substrate is placed in a plasma enhanced chemical vapor deposition (PECVD) device to sequentially grow the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer.
[0071] Wherein, the first doped layer is an oxygen-doped polysilicon layer. In other embodiments, it can also be a carbon-doped polysilicon layer, or a polysilicon layer doped with both oxygen and carbon. Wherein, doping with carbon and / or oxygen elements can reduce the parasitic absorption of the polysilicon layer. Although the introduction of carbon and / or oxygen elements will introduce damage to the tunneling layer, providing a lightly doped layer can reduce the damage to the tunneling layer.
[0072] Preferably, the thickness of the first doping layer 4 is in the range of 50-100 nanometers. For example, the thickness of the first doping layer 4 can be set to 60 millimeters. In other embodiments, the thickness of the first doping layer 4 can also be set to 80 millimeters. Of course, other thicknesses can also be used as needed.
[0073] Preferably, the thickness of the heavily doped layer 5 is in the range of 30-60 nanometers. For example, the thickness of the heavily doped layer 5 can be set to 30 millimeters. In other embodiments, the thickness of the heavily doped layer 5 can also be set to 40 millimeters. Of course, other thicknesses can also be used as needed. It should be noted that the thinner the heavily doped layer 5 is, the lower the parasitic absorption is. Therefore, under the condition of ensuring the contact resistance, the thinner the heavily doped layer 5 is, the better.
[0074] Preferably, the thickness of the lightly doped layer 3 is in the range of 5-10 nanometers. For example, the thickness of the lightly doped layer 3 can be set to 5 millimeters. In other embodiments, the thickness of the lightly doped layer 3 can also be set to 8 millimeters. Of course, other thicknesses can also be used as needed.
[0075] In step S300, the battery is annealed at high temperature, specifically, the temperature range is 820-880°C, and the time range is 10-30 minutes.
[0076] After the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer are annealed, a passivation layer is formed on the heavily doped layer using a plasma enhanced chemical vapor deposition device, and the passivation layer is activated at high temperature. The provision of the passivation layer can reduce surface defects of the solar cell, increase carrier lifetime, and prevent light corrosion. Preferably, the passivation layer is silicon nitride. In other embodiments, the passivation layer can also be aluminum oxide.
[0077] In step S400, the other surface of the silicon substrate is first subjected to a second cleaning, which may be performed by hydrofluoric acid cleaning or other cleaning methods, and then polishing is performed, followed by a third cleaning, which may be a wet chemical cleaning method.
[0078] Then, the intrinsic amorphous silicon layer and the second doped layer are sequentially formed from the other surface of the silicon substrate by chemical vapor deposition (CVD). The second doped layer is a doped amorphous silicon layer or a doped microcrystalline silicon layer.
[0079] The silicon wafer is placed in a reactive plasma deposition (RPD) setup to form the transparent conductive oxide thin film on the second doped layer, with a deposition thickness ranging from 50 to 200 nanometers.
[0080] The front and back grid lines of the battery are opened by photolithography, and then low-temperature silver paste is printed. After curing, a first electrode is formed on the heavily doped layer, and a second electrode is formed on the transparent conductive oxide film. Then light is injected to excite the battery cell.
[0081] Then, a reflection enhancement layer is deposited on the transparent conductive oxide film by evaporation. The reflection enhancement layer 11 can be made of materials with a high refractive index such as silicon or silicon dioxide to reduce the light loss reflected from the cell surface and improve the transmission and absorption of light.
[0082] The solar cell manufacturing method of this embodiment is used to manufacture the solar cell, which can reduce the optical loss of the solar cell, help reduce the composite current density of the solar cell, and improve the conversion efficiency of the solar cell.
[0083] In one of the embodiments, the method for preparing a solar cell of this embodiment is used to prepare the solar cell described in any one of the embodiments of the first aspect above.
[0084] An embodiment of a third aspect of the present invention provides a photovoltaic module.
[0085] The photovoltaic assembly includes a plurality of solar cells connected in series and / or in parallel. The structure of the solar cell is the same as the structure of the solar cell described in any one of the embodiments of the first aspect above, and will not be described in detail here.
[0086] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A solar cell, characterized in that: comprising a silicon substrate, a first surface and a second surface; The first surface and the second surface are arranged opposite to each other; A tunneling layer, a lightly doped layer, a first doped layer and a heavily doped layer are sequentially provided between the silicon substrate and the first surface starting from the silicon substrate, wherein the first doped layer is doped with at least one element of oxygen or carbon; An intrinsic amorphous silicon layer is disposed between the silicon substrate and the second surface.
2. The solar cell according to claim 1, characterized in that The first doped layer is an oxygen-doped polysilicon layer, a carbon-doped polysilicon layer, or a polysilicon layer doped with both oxygen and carbon.
3. The solar cell according to claim 1, characterized in that The thickness of the first doping layer is in the range of 50-100 nanometers.
4. The solar cell according to claim 1, characterized in that The heavily doped layer has a thickness ranging from 30 to 60 nanometers.
5. The solar cell according to claim 1, characterized in that: The thickness of the lightly doped layer is in the range of 5-10 nanometers.
6. The solar cell according to claim 1, characterized in that The first surface is a light-facing surface of the solar cell, and the second surface is a light-backed surface of the solar cell.
7. The solar cell according to claim 1, characterized in that A passivation layer and a first electrode are disposed on the heavily doped layer. The first electrode is connected to the heavily doped layer. The passivation layer covers the heavily doped layer and exposes the first electrode.
8. The solar cell according to claim 7, characterized in that: The passivation layer is silicon nitride or aluminum oxide.
9. The solar cell according to claim 1, characterized in that: The intrinsic amorphous silicon layer is intrinsic amorphous silicon containing oxygen, intrinsic amorphous silicon containing carbon, or intrinsic amorphous silicon containing nitrogen.
10. The solar cell according to claim 1, characterized in that: A second doping layer is further disposed between the intrinsic amorphous silicon layer and the second surface, and the doping type of the second doping layer is opposite to that of the silicon substrate.
11. The solar cell according to claim 10, characterized in that The second doped layer is a doped amorphous silicon layer or a doped microcrystalline silicon layer.
12. The solar cell according to claim 1, characterized in that The silicon substrate, the lightly doped layer and the heavily doped layer are all N-type doped.
13. The solar cell according to claim 1, characterized in that A transparent conductive oxide film is further arranged between the intrinsic amorphous silicon layer and the second surface, a second electrode is arranged on the transparent conductive oxide film, and the transparent conductive oxide film is connected to the second electrode.
14. The solar cell according to claim 13, characterized in that: The invention also includes a reflection enhancement layer, which covers the transparent conductive oxide film and exposes the second electrode.
15. A method for preparing a solar cell, characterized in that: include: providing a silicon substrate; Forming a tunneling layer, a lightly doped layer, a first doped layer and a heavily doped layer in sequence from one surface of the silicon substrate, and doping the first doped layer with at least one element of oxygen or carbon; Performing annealing treatment on the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer; An intrinsic amorphous silicon layer is formed on the other surface of the silicon substrate.
16. The method for preparing a solar cell according to claim 15, characterized in that: Before forming the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer, the silicon substrate is textured and first cleaned.
17. The method for preparing a solar cell according to claim 15, characterized in that: After the tunneling layer, the lightly doped layer, the first doped layer and the heavily doped layer are annealed, a passivation layer is formed on the heavily doped layer, and the passivation layer is activated.
18. The method for preparing a solar cell according to claim 15, characterized in that: The other surface of the silicon substrate is cleaned for the second time, then polished, and then cleaned for the third time to form the intrinsic amorphous silicon layer; a second doped layer is formed on the intrinsic amorphous silicon layer, a transparent conductive oxide film is formed on the second doped layer, a first electrode is formed on the heavily doped layer, and a second electrode is formed on the transparent conductive oxide film.
19. The method for preparing a solar cell according to claim 18, characterized in that: A reflection enhancement layer is formed on the transparent conductive oxide film and the second electrode is exposed.
20. A photovoltaic module, characterized in that: The invention comprises a plurality of solar cells according to any one of claims 1 to 14 connected in series and / or in parallel.
Citation Information
Cited By
Tunneling passivation contact structure and preparation method thereof, solar cell and photovoltaic module
CN120614908A