Lithium ferric manganese phosphate coated lithium-rich manganese-based composite positive electrode material and preparation and application thereof
By coating lithium manganese phosphate and carbon layer on the lithium-rich manganese-based positive electrode material to form a multi-layer structure, the problem of insufficient voltage drop and cycle life is solved, the high voltage and high energy density are achieved, and the production is reduced cost.
Patent Information
- Application Number
- CN202411036986.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The existing lithium-rich manganese-based positive electrode materials have problems such as voltage drop, insufficient cycle life and decreased energy density, and lithium manganese iron phosphate composite materials are unstable under high voltage and cannot fully utilize the advantages of high voltage.
The multi-layer structure design is designed to coat the lithium-rich manganese-based composite positive electrode material with lithium-rich manganese-based composite material. The inner layer is lithium-rich manganese-phosphate, the secondary outer layer is lithium-manganese-phosphate, and the outer layer is carbon material. Through the optimization preparation process and constant current Constant voltage charging and discharging strategy to improve material stability and voltage retention.
It significantly improves voltage retention rate and cycle stability, extends battery life, solves the problems of voltage drop and energy density reduction, and reduces production costs and achieves large-scale production.
Smart Images

Figure CN118969999A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries, and in particular relates to a lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material and a preparation method and application thereof. Background Art
[0002] The ever-increasing energy consumption in modern society requires energy storage technologies with ever-increasing energy density. Lithium-ion batteries (LIBs) have always been the mainstream energy storage technology for mobile applications, and are also considered to be the most suitable technology for electric vehicles and stationary energy storage systems. The current mainstream positive electrode materials are mainly divided into two categories: one is the transition metal oxide type positive electrode material, typically represented by LiCoO2; the second is the polyanion compound type positive electrode material, typically represented by LiFePO4. Both of these categories are lithium ion embedding materials, and the valence state of the transition metal changes during the lithium ion deintercalation process. The theoretical capacity of LiCoO2 is close to 280mAhg -1 , which means that the maximum capacity that can be provided by extracting all the Li in the structure is as Li + Escape, Li + The interaction between the O atoms on both sides is weakened, the electrostatic repulsion between the layers gradually increases, and the internal stress increases, causing the LiCoO2 layer to slip, collapse, and even irreversible structural changes to the spinel phase. In practical applications, the capacity of early lithium cobalt oxide can only be half. LiFePO4 is considered to be one of the most promising positive electrode materials. It has the advantages of good structural stability, long cycle life, low cost, environmental friendliness, and good safety. However, the electronic conductivity of LiFePO4 (~10 at room temperature) is -9 The low S / cm) has led researchers to solve this problem through different approaches.
[0003] In 1997, Numata et al. first reported the solid solution structure of LiCoO2-Li2MnO3. We usually call it lithium-rich manganese-based layered material. In fact, Li[Li x Ni y Co z Mn k ]O2 is a mixture of a certain amount of Li2MnO3 and ordinary layered material LiMO2. Because Li2MnO3 and LiMO2 are both α-NaFeO2 layered structures, they belong to the hexagonal system and R-3m space group. Li[Li x Ni y Co z Mn k ]O2 shows very high capacity, and the common actual capacity can reach 250-300mAhg in the charge and discharge range of 2.0-4.8V. -1Although lithium-rich cathode materials have the advantages of high reversible capacity and low cost, they also have disadvantages such as low initial coulombic efficiency, severe voltage decay and insufficient cycle life, which seriously restrict the application of lithium-rich cathode materials in practice.
[0004] Lithium manganese iron phosphate has the same olivine crystal structure as lithium iron phosphate. Lithium iron phosphate has become the most commercially valuable cathode material due to its advantages such as green environmental protection, good safety, low raw material cost and high abundance, and stable structure. It is widely used in power and energy storage scenarios. Lithium manganese iron phosphate has a higher voltage platform than lithium iron phosphate, and its energy density is increased by more than 20%, which has a very broad application prospect. However, lithium manganese iron phosphate still has problems such as poor electronic conductivity, low lithium ion diffusion coefficient, and the Jan-Taylor effect of Mn, especially during the charge and discharge process. 2+ It will dissolve and deposit on the negative electrode, seriously deteriorating the battery cycle performance. Therefore, the advantages can be achieved by combining the two in different proportions.
[0005] For example, Chinese patents CN103682318A and CN104201366A utilize the high safety performance of ternary materials and compound lithium iron phosphate with ternary materials during the homogenization process. In addition to the same material uniformity problem as in the above two patents, since the energy density of lithium iron phosphate is lower than that of ternary materials, the energy density of the mixed electrode after compounding is reduced, that is, the improvement in performance is at the expense of energy density.
[0006] Patent CN114256448A discloses a lithium-rich manganese iron phosphate composite material, which ensures the capacity of the material, but the composite material reduces the advantage of high working voltage of lithium-rich materials, and lithium-rich manganese iron phosphate becomes unstable under high voltage. At the same time, the serious voltage drop problem of lithium-rich materials has not been solved, and a charging and discharging mode is urgently needed to solve the shortcomings between the two and maximize the synergistic effect. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention provides a lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material and its preparation and application. The composite positive electrode material prepared by the present invention is a multilayer structure, the innermost layer is a lithium-rich manganese-based, the second outermost layer is a lithium iron manganese phosphate material, and the outermost layer is a carbon material. This multilayer structure not only takes advantage of the high specific capacity of the lithium-rich material, but also increases the stability of the lithium-rich manganese-based positive electrode material. The obtained composite positive electrode effectively improves the serious voltage drop problem of the traditional lithium-rich manganese-based positive electrode material. In particular, after optimizing the constant current and constant voltage test conditions, the composite positive electrode has a good performance at 1C (1C = 250mAh g -1 ) current, the voltage holding rate can be increased from 78.55% to over 85% after 500 cycles.
[0008] In order to solve the problems of the prior art, the technical solution adopted by the present invention is:
[0009] A lithium-rich manganese-based composite cathode material coated with lithium iron manganese phosphate, wherein the lithium iron manganese phosphate-coated lithium-rich manganese-based composite cathode material has a multi-layer structure, and from the inside to the outside are a lithium-rich manganese base layer, a lithium iron manganese phosphate layer coated on the lithium-rich manganese base layer, and a carbon layer outside the lithium iron manganese phosphate layer.
[0010] As an improvement, the thicknesses of the lithium iron manganese phosphate layer and the carbon layer are 300 to 600 nm.
[0011] The preparation method of the above-mentioned lithium iron manganese phosphate-coated lithium-rich manganese-based composite cathode material includes the following steps:
[0012] Step 1, uniformly mix the precursor and the lithium source according to a molar ratio of 1:0.5 to 1.5, and first heat it to 400 to 550 °C in a muffle furnace under an air atmosphere at a heating rate of 1 to 10 °C min -1 and keep it warm for 3 to 7 h, then heat it to 700 to 1000 °C and keep it warm for 5 to 20 h, and then cool it naturally to obtain a lithium-rich manganese-based material with a molecular formula of Li[Li x Ni y Co z Mn k O2, where 0.07 ≤ x ≤ 0.26, 0 < y ≤ 0.23, 0 < z ≤ 0.17, 0.43 ≤ k ≤ 0.68;
[0013] Step 2, mix the lithium iron manganese phosphate and the carbon source according to a mass ratio, and grind them充分 to obtain a carbon-coated lithium iron manganese phosphate material. Among them, the molecular formula of lithium iron manganese phosphate is LiMn a Fe b N c PO4, where 0 < a ≤ 0.6, 0 < b ≤ 1, 0 < c ≤ 0.6, and N is one or more combinations of Cr, Cu, Al, Nb, Ti, or Co;
[0014] Step 3, mix the carbon-coated lithium iron manganese phosphate and the lithium-rich manganese base according to a mass ratio, and grind them充分 to obtain a composite cathode material with a multi-layer structure; or after grinding, heat it to 50 to 300 °C under gas protection and keep it warm for 0 to 10 h to obtain a composite cathode material with a multi-layer structure.
[0015] As an improvement, the precursor in Step 1 is Mn m Co n Ni g T s (OH)2 or Mn m Co n Ni g T sCO3, where 0 < g ≤ 0.4, 0 < n ≤ 0.45, 0 < m ≤ 0.75, 0 ≤ s ≤ 0.2, and T is one or a combination of Mg, Al, Ca, V, Mo, Fe, Nb, or Zr; the lithium source is one or a mixture of Li2CO3 or LiOH·H2O.
[0016] As an improvement, the step 1 further includes doping with metal oxides, and the formula of the lithium-rich manganese-based material is Li[Li x Ni y Co z Mn k M d O2, where M is a doping element, and 0.07 ≤ x ≤ 0.25, 0 < y ≤ 0.22, 0 < z ≤ 0.16, 0.43 ≤ k ≤ 0.65, 0 < d ≤ 0.05.
[0017] Further improvement is that the doping metal oxide is one or a mixture of MgO, Al2O3, TiO2, ZrO2, Nb2O5, Fe2O3, ZnO, CaO, V2O5, MoO3, WO3, or CuO.
[0018] As an improvement, in step 2, the mass of the carbon source accounts for 1 - 10% of the total mass of lithium iron phosphate and the carbon source, the particle size of lithium iron phosphate is 300 - 600 nm, and the carbon source is one or a combination of amorphous carbon, hard carbon, graphene, carbon nanotubes, polyvinylpyrrolidone.
[0019] As an improvement, in step 3, the mass of the carbon-coated lithium iron phosphate accounts for 2 - 98% of the total mass of the composite cathode material, the particle size of the lithium-rich manganese-based material is 2 - 20 μm, and the protective gas is nitrogen, oxygen, or argon.
[0020] The application of the above lithium iron phosphate-coated lithium-rich manganese-based composite cathode material in the preparation of lithium-ion batteries.
[0021] As an improvement, the current in the constant current (CC) stage of the lithium-ion battery is 0.1 - 10C; the constant voltage (CV) is 4.4 - 4.7V; the current magnitude under constant voltage (CV) is 0.1 - 0.5 times that of the constant current (CC).
[0022] Compared with the prior art, the lithium iron phosphate-coated lithium-rich manganese-based composite cathode material and its preparation and application of the present invention have the following advantages:
[0023] (1) The lithium iron manganese phosphate coated lithium-rich manganese base of the present invention has a lithium-rich manganese base as a core, lithium iron manganese phosphate and carbon as an outer shell, and the lithium-rich manganese base is sintered. By mixing the carbon-containing lithium iron manganese phosphate and the lithium-rich manganese base, the lithium iron manganese phosphate is uniformly and densely coated on the surface of the lithium-rich manganese base material to form a uniform and dense coating shell, which can not only give full play to the high voltage and high capacity of the lithium-rich manganese base material, and target masking to unlock the stable performance of the lithium-rich material at 4.8V, but also give full play to the long cycle characteristics of lithium iron manganese phosphate, improve the high temperature performance and high temperature cycle performance of lithium iron manganese phosphate, so that the obtained lithium iron manganese phosphate coated lithium-rich manganese base composite positive electrode material has both high capacity and stability, and then the cycle performance and rate performance of the lithium ion battery prepared by it can be greatly improved.
[0024] (2) The present invention provides an optimized constant current and constant voltage charging strategy to solve the problem that the lithium-rich manganese-based composite positive electrode material coated with lithium iron manganese phosphate cannot take advantage of the high voltage, and solves the serious voltage drop problem of lithium-rich materials and the problem of reduced energy density of the battery when the charging cut-off voltage is reduced. In the CV step, the battery is charged at a constant voltage until the current drops to the set value, the extra lithium ions are removed from the cathode particles, and the uneven distribution of lithium inside the cathode is alleviated.
[0025] (3) The preparation method of the lithium-rich manganese-based composite positive electrode material coated with lithium manganese iron phosphate by mixing is simple and efficient, does not introduce any impurities, has low production costs, and can achieve large-scale production.
[0026] (4) The lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material of the present invention not only improves the discharge specific capacity and cycle stability, but also significantly suppresses the most serious voltage drop problem of the lithium-rich manganese-based composite positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a SEM image of the lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 of the present invention;
[0028] Figure 2 This is a SEM image of the lithium iron manganese phosphate of Example 1 of the present invention;
[0029] Figure 3 This is a SEM image of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 1 of the present invention;
[0030] Figure 4 This is a SEM image of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 2 of the present invention;
[0031] Figure 5 XRD patterns of the lithium-rich manganese-based positive electrode material, lithium iron manganese phosphate, and lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Comparative Example 1 and Example 1 of the present invention;
[0032] Figure 6 This is a graph showing the voltage retention rate of the lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 of the present invention under constant current and constant voltage;
[0033] Figure 7 The lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 of the present invention is subjected to a constant current of 1C (1C = 250 mAh g -1 ) Voltage holding rate diagram of 2.0~4.8V;
[0034] Figure 8 The lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material prepared in Comparative Example 2 of the present invention was heated at a constant current of 1C (1C = 250 mAh g -1 ) Voltage holding rate diagram of 2.0~4.8V;
[0035] Fig. 9 This is a graph showing the voltage retention rate of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 1 of the present invention under constant current and constant voltage;
[0036] Fig.10 This is a graph showing the voltage retention rate of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 2 of the present invention under constant current and constant voltage;
[0037] Fig.11 This is a graph showing the voltage retention rate of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 3 of the present invention under constant current and constant voltage;
[0038] Fig.12 This is a graph showing the voltage retention rate of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 4 of the present invention under constant current and constant voltage;
[0039] Fig.13 This is a graph showing the voltage retention rate of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 5 of the present invention under constant current and constant voltage;
[0040] Fig.14 This is a graph showing the voltage retention rate of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 6 of the present invention under constant current and constant voltage;
[0041] Fig.15 This is a graph showing the voltage retention rate of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 7 of the present invention under constant current and constant voltage;
[0042] Fig.16 The energy density retention rate diagram of the lithium-rich and lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode materials prepared in Example 5 of the present invention and Comparative Example 1 and Comparative Example 2;
[0043] Fig.17A comparison chart of the voltage retention rates of lithium-rich and lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode materials prepared in Example 5 of the present invention and Comparative Example 1 and Comparative Example 2;
[0044] Fig.18 It is a comparison chart of the capacity retention rate of lithium-rich and lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode materials prepared in Comparative Example 1, Example 3 and Example 4 of the present invention;
[0045] Fig.19 This is a comparison chart of the capacity retention rates of the lithium-rich and lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode materials prepared in Comparative Example 1 and Example 8 of the present invention at high temperatures. DETAILED DESCRIPTION
[0046] The technical solution of the present invention is further described below in conjunction with embodiments.
[0047] The present invention Mn 0.675 Co 0.1625 Ni 0.1625 CO3、Mn 0.575 Co 0.1625 Ni 0.1625 Mo 0.05 Fe 0.05 CO3、Mn 0.675 Co 0.1625 Ni 0.1625 (OH)2 precursor, LiMn 0.35 Fe 0.6 Co 0.05 PO4、LiMn 0.4 Fe 0.6 PO4、LiMn 0.35 Fe 0.6 Al 0.05 PO4 was purchased from Haian Intelligent Battery Material Technology Co., Ltd.
[0048] The carbon sources of the present invention are amorphous carbon and hard carbon, both of which are purchased from Zhejiang Yamei Nano Technology Co., Ltd.
[0049] The preparation methods of the button batteries in the embodiments of the present invention and comparative examples 1 to 2 are as follows:
[0050] First, lithium iron manganese phosphate is coated with a lithium-rich manganese-based composite positive electrode material or a lithium-rich manganese-based positive electrode material Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2 is mixed with Super P and PVDF in a molar ratio of 8:1:1. After being fully ground, an appropriate amount of N-methyl-di-ethylpyrrolidone is added as a solvent, mixed to form a uniform slurry, coated on the surface of aluminum foil, and dried.
[0051] Secondly, after the slurry is completely dried, the aluminum foil is cut into round pieces (Φ=11 mm) and the mass is weighed and recorded.
[0052] Finally, the electrode pieces are assembled in the order of positive electrode shell, electrode piece, diaphragm, lithium sheet, gasket, shrapnel and negative electrode shell to form a button battery.
[0053] Example 1
[0054] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.35 Fe 0.6 Co 0.05 PO4, the preparation method comprises the following steps:
[0055] Mn 0.675 Co 0.1625 Ni 0.1625 The CO3 precursor and Li2CO3 were mixed evenly in a molar ratio of 1:1.33 and heated at 5 °C min -1 The temperature was first raised to 450 °C in a muffle furnace in an air atmosphere for 5 h, then raised to 800 °C for 8 h, and then naturally cooled to room temperature to obtain a lithium-rich manganese-based cathode material Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2.
[0056] According to C:LiMn 0.35 Fe 0.6 Co 0.05 PO4=1:10 mass ratio, mix hard carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.35 Fe 0.6 Co 0.05 PO4 / C.
[0057] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.35 Fe 0.6 Co 0.05 PO4 / C:Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2=1:9 mass ratio, fully grind, and finally in oxygen atmosphere at 5℃min -1 The temperature was raised to 300°C at a rate and kept warm for 5 hours to obtain a multi-layered composite positive electrode material.
[0058] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles of activation every 50 cycles, the voltage range is 2-4.5V, and after reaching 4.5V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.5V, and after reaching 4.5V, constant voltage charging is performed until the current drops to 0.2C.
[0059] Example 2
[0060] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.46 Mo 0.04 Fe 0.04 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.4 Fe 0.6 PO4, including the following steps:
[0061] Mn 0.575 Co 0.1625 Ni 0.1625 Mo 0.05 Fe 0.05 The CO3 precursor and Li2CO3 were mixed evenly in a molar ratio of 1:1.33 and heated at 5 °C min -1 The temperature was first raised to 450 °C in an air atmosphere in a muffle furnace and kept for 5 h, then raised to 800 °C and kept for 8 h, and then naturally cooled to room temperature to obtain the lithium-rich manganese-based material Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.46 Mo 0.04 Fe 0.04 ]O2.
[0062] According to C:LiMn 0.4 Fe 0.6 PO4=1:10 mass ratio, mix amorphous carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.4 Fe 0.6 PO4 / C.
[0063] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.4 Fe 0.6 PO4 / C:Li[Li 0.2 Ni0.13 Co 0.13 Mn 0.46 Mo 0.04 Fe 0.04 ]O2=1:4.55 mass ratio, fully grind, and finally in nitrogen atmosphere at 5℃min -1 The temperature was raised to 300°C at a rate and kept warm for 5 hours to obtain a multi-layered composite positive electrode material.
[0064] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.5V, after reaching 4.5V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.5V, after reaching 4.5V, constant voltage charging is performed until the current drops to 0.2C.
[0065] Example 3
[0066] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.4 Fe 0.6 PO4, the preparation method comprises the following steps:
[0067] Mn 0.675 Co 0.1625 Ni 0.1625 The CO3 precursor and Li2CO3 were mixed evenly in a molar ratio of 1:1.33 and heated at 5 °C min -1 The temperature was first raised to 450 °C in an air atmosphere in a muffle furnace and kept for 5 h, then raised to 800 °C and kept for 8 h, and then naturally cooled to room temperature to obtain the lithium-rich manganese-based material Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2.
[0068] According to C:LiMn 0.4 Fe 0.6 PO4=1:11.5 mass ratio, mix amorphous carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.4 Fe 0.6 PO4 / C.
[0069] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.4 Fe 0.6 PO4 / C:Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2=1:3 mass ratio, fully grind, and finally in nitrogen atmosphere at 5℃min -1 The temperature was raised to 300°C at a rate and kept warm for 5 hours to obtain a multi-layered composite positive electrode material.
[0070] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.55V, after reaching 4.55V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.55V, after reaching 4.55V, constant voltage charging is performed until the current drops to 0.2C.
[0071] Example 4
[0072] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.12 Co 0.12 Mn 0.54 Ca 0.02 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.35 Fe 0.6 Al 0.05 PO4, including the following steps:
[0073] Mn 0.675 Co 0.1625 Ni 0.1625 The CO3 precursor, Li2CO3 and CaO were mixed in a molar ratio of 39:30:1 and heated at 5 °C min -1 The temperature was first raised to 450 °C in an air atmosphere in a muffle furnace and kept for 5 h, then raised to 800 °C and kept for 8 h, and then naturally cooled to room temperature to obtain the lithium-rich manganese-based material Li[Li 0.2 Ni 0.12 Co 0.12 Mn 0.54 Ca 0.02 ]O2.
[0074] According to C:LiMn 0.35 Fe0.6 Al 0.05 PO4=1:9 mass ratio, mix amorphous carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.35 Fe 0.6 Al 0.05 PO4 / C.
[0075] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.35 Fe 0.6 Al 0.05 PO4 / C:Li[Li 0.2 Ni 0.12 Co 0.12 Mn 0.54 Ca 0.02 ]O2=1:9 mass ratio, fully grind, and finally in nitrogen atmosphere at 5℃min -1 The temperature was raised to 300°C at a rate and kept warm for 5 hours to obtain a multi-layered composite positive electrode material.
[0076] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.7V, after reaching 4.7V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.7V, after reaching 4.7V, constant voltage charging is performed until the current drops to 0.2C.
[0077] Example 5
[0078] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.1235 Co 0.1235 Mn 0.513 Nb 0.04 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.4 Fe 0.6 PO4, including the following steps:
[0079] Mn 0.675 Co 0.1625 Ni 0.1625 The (OH)2 precursor, Li2CO3 and Nb2O5 were uniformly mixed in a molar ratio of 38:30:1 and heated at 5 °C min -1The temperature was first raised to 500 °C in an air atmosphere in a muffle furnace at a heating rate of 500 °C for 5 h, then raised to 900 °C for 8 h, and then naturally cooled to room temperature to obtain the lithium-rich manganese-based material Li[Li 0.2 Ni 0.1235 Co 0.1235 Mn 0.513 Nb 0.04 ]O2.
[0080] According to C:LiMn 0.4 Fe 0.6 PO4=1:11.5 mass ratio, mix amorphous carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.4 Fe 0.6 PO4 / C.
[0081] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.4 Fe 0.6 PO4 / C:Li[Li 0.2 Ni 0.1235 Co 0.1235 Mn 0.513 Nb 0.04 ]O2=1:1 mass ratio, fully grind, and finally in nitrogen atmosphere at 5℃min -1 The temperature was raised to 300°C at a rate and kept warm for 5 hours to obtain a multi-layered composite positive electrode material.
[0082] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.5V, after reaching 4.5V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.5V, after reaching 4.5V, constant voltage charging is performed until the current drops to 0.2C.
[0083] Example 6
[0084] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.4 Fe 0.6 PO4, the preparation method comprises the following steps:
[0085] Mn0.675 Co 0.1625 Ni 0.1625 The CO3 precursor and Li2CO3 were mixed evenly in a molar ratio of 1:1.33 and heated at 5 °C min -1 The temperature was first raised to 450 °C in an air atmosphere in a muffle furnace and kept for 5 h, then raised to 800 °C and kept for 8 h, and then naturally cooled to room temperature to obtain the lithium-rich manganese-based material Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2.
[0086] According to C:LiMn 0.4 Fe 0.6 PO4=1:11.5 mass ratio, mix amorphous carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.4 Fe 0.6 PO4 / C.
[0087] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.4 Fe 0.6 PO4 / C:Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2=1:3 mass ratio is mixed and fully ground to obtain a composite positive electrode material with a multi-layer structure.
[0088] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.55V, after reaching 4.55V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.55V, after reaching 4.55V, constant voltage charging is performed until the current drops to 0.2C.
[0089] Example 7
[0090] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.4 Fe 0.6 PO4, the preparation method comprises the following steps:
[0091] Mn 0.675 Co 0.1625 Ni 0.1625 The CO3 precursor and Li2CO3 were mixed evenly in a molar ratio of 1:1.33 and heated at 5 °C min -1 The temperature was first raised to 450 °C in an air atmosphere in a muffle furnace and kept for 5 h, then raised to 800 °C and kept for 8 h, and then naturally cooled to room temperature to obtain the lithium-rich manganese-based material Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2.
[0092] According to C:LiMn 0.4 Fe 0.6 PO4=1:11.5 mass ratio, mix amorphous carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.4 Fe 0.6 PO4 / C.
[0093] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.4 Fe 0.6 PO4 / C:Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2=49:1 mass ratio is mixed and fully ground to obtain a composite positive electrode material with a multi-layer structure.
[0094] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.55V, after reaching 4.55V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.55V, after reaching 4.55V, constant voltage charging is performed until the current drops to 0.2C.
[0095] Example 8
[0096] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.4 Fe 0.6 PO4, the preparation method comprises the following steps:
[0097] Mn 0.675 Co 0.1625 Ni 0.1625 The CO3 precursor and Li2CO3 were mixed evenly in a molar ratio of 1:1.33 and heated at 5 °C min -1 The temperature was first raised to 450 °C in an air atmosphere in a muffle furnace and kept for 5 h, then raised to 800 °C and kept for 8 h, and then naturally cooled to room temperature to obtain the lithium-rich manganese-based material Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2.
[0098] According to C:LiMn 0.4 Fe 0.6 PO4=1:11.5 mass ratio, mix amorphous carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.4 Fe 0.6 PO4 / C.
[0099] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.4 Fe 0.6 PO4 / C:Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2=1:3 mass ratio, fully grind, and finally in nitrogen atmosphere at 5℃min -1 The temperature was raised to 300°C at a rate and kept warm for 5 hours to obtain a multi-layered composite positive electrode material.
[0100] The battery was tested for charge and discharge cycles at 50°C using a tester (CT2001A) produced by Blue Electric. The test channel range was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.55V, after reaching 4.55V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.55V, after reaching 4.55V, constant voltage charging is performed until the current drops to 0.2C.
[0101] Comparative Example 1
[0102] The lithium-rich manganese-based positive electrode material prepared in Example 1 has a molecular formula of Li[Li 0.2 Ni 0.13 Co 0.13 Mn0.54 ]O2, as comparative example 1.
[0103] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.5V, after reaching 4.5V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.5V, after reaching 4.5V, constant voltage charging is performed until the current drops to 0.2C.
[0104] Comparative Example 2
[0105] The molecular formula of lithium-rich manganese-based cathode material is Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2, the molecular formula of lithium manganese iron phosphate is LiMn 0.4 Fe 0.6 PO4
[0106] Mn 0.675 Co 0.1625 Ni 0.1625 The CO3 precursor and Li2CO3 were mixed evenly in a molar ratio of 1:1.33 and heated at 5 °C min -1 The temperature was first raised to 450 °C in an air atmosphere in a muffle furnace and kept for 5 h, then raised to 800 °C and kept for 8 h, and then naturally cooled to room temperature to obtain the lithium-rich manganese-based material Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2.
[0107] According to C:LiMn 0.4 Fe 0.6 PO4=1:11.5 mass ratio, mix amorphous carbon with lithium iron manganese phosphate, grind thoroughly, and obtain carbon-coated lithium iron manganese phosphate material LiMn 0.4 Fe 0.6 PO4 / C.
[0108] Then, the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese-based LiMn 0.4 Fe 0.6 PO4 / C:Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54]O2=1:1 mass ratio, fully grind, and finally in nitrogen atmosphere at 5℃min -1 The temperature was raised to 300°C at a rate and kept warm for 5 hours to obtain a multi-layered composite positive electrode material.
[0109] The battery was tested for charge and discharge cycles at room temperature (25°C) using a tester (CT2001A) produced by Blue Electric. The test channel range used was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current is used to activate the battery twice every 50 cycles, with a voltage range of 2 to 4.8 V. Then, a cycle test is performed at a constant current of 1C, with a voltage range of 2 to 4.8 V.
[0110] Comparative Example 3
[0111] The lithium-rich manganese-based positive electrode material prepared in Example 1 has a molecular formula of Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2, as comparative example 3.
[0112] The battery was tested for charge and discharge cycles at 50°C using a tester (CT2001A) produced by Blue Electric. The test channel range was 5V, 10mA, and the recording time was 10s. The specific test conditions were: after the assembled button battery was left to stand for 1 day, the battery was charged and discharged using a 0.1C (1C = 250mAh g -1 ) constant charge and discharge current for two cycles every 50 cycles, the voltage range is 2-4.5V, after reaching 4.5V, constant voltage charging is performed until the current drops to 0.02C. Secondly, a constant current 1C cycle test is performed, the voltage range is 2-4.5V, after reaching 4.5V, constant voltage charging is performed until the current drops to 0.2C.
[0113] Figure 1 The lithium-rich manganese-based positive electrode material (Li[Li 0.2 Ni 0.13 Co 0.13 Mn 0.54 ]O2) SEM image, Figure 2 This is a SEM image of the lithium manganese iron phosphate of Example 1. Figures 1-2 It can be observed that the lithium-rich manganese-based positive electrode material and lithium iron manganese phosphate particles prepared by the method of the present invention are dispersed, the particle size of the lithium-rich manganese-based positive electrode material is 2 to 20 μm, and the particle size of the lithium iron manganese phosphate is 300 to 600 nm.
[0114] Figure 3This is a SEM image of the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material prepared in Example 1 of the present invention. Figure 4 This is a SEM image of the lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material prepared in Example 2. Figure 3-4 It can be observed that the lithium iron manganese phosphate prepared by the method of the present invention wraps the lithium-rich manganese-based composite positive electrode material, and the lithium iron manganese phosphate and the carbon layer are sequentially stacked and coated on the surface of the lithium-rich manganese-based material, which can perfectly avoid the risk of the lithium-rich material coming into contact with the air or reaction solvent, reduce the material storage cost and the process cost of material processing, while taking into account the performance effect, overcoming the disadvantage of insufficient conductivity, and improving the voltage retention of the material.
[0115] Figure 5 The XRD of the lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 of the present invention and the lithium-rich manganese-based composite positive electrode material coated with lithium iron manganese phosphate prepared in Example 1. It can be seen from the figure that the diffraction peak is basically consistent with the lithium-rich material standard card, and in the range of 20° to 25°, the existence of superlattice peaks can be observed, and the XRD spectrum shows a two-phase structure of LiMO2 layered phase and Li2MnO3 monoclinic phase. Among them, the XRD of the lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material prepared in Example 1 also corresponds to the diffraction peaks of lithium iron manganese phosphate and lithium-rich manganese-based, respectively.
[0116] Combination Figure 1 to Figure 5 The SEM and XRD characterization results confirm that the present invention successfully produces a uniformly dispersed lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material.
[0117] In the blue electricity test system, the charge and discharge test was completed at room temperature, high temperature, and voltage range under the conditions of different embodiments. The test results are as follows Figures 6 to 19 shown.
[0118] Figures 6-7 This is a performance test of the lithium-rich manganese-based positive electrode material prepared in Example 1. It can be seen from the figure that under the constant current condition of 2-4.8V, the layered structure of the lithium-rich manganese-based positive electrode material changes to rock salt and spinel structure, and the transition metal valence state continues to decrease during the cycle, the median voltage of the lithium-rich manganese-based positive electrode material continues to decrease, and the voltage holding rate also decreases accordingly. Under constant current and constant voltage, the voltage holding rate is alleviated to a certain extent.
[0119] It can be seen that under the optimized constant current and constant voltage charge and discharge strategy, the lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material of the present invention will not only not reduce the energy density due to the decrease in voltage margin, but also extend the life of the battery and reduce polarization.
[0120] Figures 8 to 19The lithium-rich manganese-based positive electrode material is prepared by wrapping lithium manganese iron phosphate with precursors of different molar ratios, and Examples 1 to 8 and Comparative Examples 1 to 3 are prepared by changing the content of iron, manganese, doping elements, outer carbon layer wrapped in lithium manganese iron phosphate, test temperature and other factors. In Example 3, the lithium-rich manganese-based composite positive electrode material wrapped with lithium manganese iron phosphate is subjected to constant current and constant voltage of 1C (1C = 250mAh g -1 ) at a current density of 83.14% (500 cycles), showing good voltage retention, while the comparative examples 1 and 2 showed good voltage retention at 1C (1C = 250 mAh g -1 ) at a current density of 77.34% and 82.94% (500 cycles). The improvement in voltage retention is directly reflected in the energy density, which increases from 60.59% in comparative example 1 to 72.36% in example 3 (500 cycles). In example 1, 5% Co is introduced into the lithium manganese iron phosphate material, and at 1C (1C = 250 mAh g -1 ) is increased from 83.14% (500 cycles) in Example 3 to 87.61%, indicating that doping a certain amount of elements in lithium manganese iron phosphate can inhibit the oxidation activity of oxygen ions on the surface of the material under high voltage, slow down the side reaction between the material and the organic electrolyte, and stabilize the surface of the material. In Example 2, 4% Mo and 4% Fe are simultaneously introduced into the lithium-rich manganese-based positive electrode material precursor, and 4% Nb is introduced in Example 5. At 1C (1C = 250 mAh g -1 ), the voltage retention rates are also improved to 87.50% and 87.71% respectively, and the capacity retention is also improved from 50.81% in Comparative Example 1 to 78.71% in Example 4, indicating that active element doping can suppress phase change and improve the capacity retention rate of the battery while maintaining the voltage retention rate.
[0121] Depend on Fig.14 It can be seen that in Example 6, the mixture of lithium manganese iron phosphate and lithium-rich manganese matrix was not sintered and the same constant current and constant voltage was obtained at 1C (1C = 250 mAh g -1 ) at a current density of 800 mAh g / cm2. The voltage holding rate was increased to 86.62% (500 cycles). In Example 7, the amount of lithium manganese iron phosphate coating was increased to 1C (1C = 250 mAh g / cm2). -1 ), the 500-cycle voltage retention rate is also increased to 86.92%, which further illustrates that the composite of lithium iron manganese phosphate and rich lithium can reversely improve the performance of lithium iron manganese phosphate as a lithium supplement. Fig.15 .
[0122] Depend on Fig.18 It can be obtained that in Example 4, Ca is doped into the lithium-rich manganese matrix and Al is doped into the carbon-coated lithium manganese iron phosphate. -1) at a current density of 50.81%, the capacity retention rate was increased from 50.81% for the unmodified lithium-manganese-rich base to 75.59% (500 cycles) after lithium iron manganese phosphate coated lithium-manganese-rich base, further indicating that doping elements in both lithium iron manganese phosphate and lithium-manganese-rich positive electrode materials can further improve the cycle stability. This indicates that lithium iron manganese phosphate coated lithium-manganese-rich composite positive electrode materials can alleviate or inhibit the side reaction between the lithium-manganese-rich positive electrode material and the electrolyte, reduce bulk oxygen loss, and effectively solve the most serious voltage drop problem of lithium-manganese-rich positive electrode materials under constant current and constant voltage. Fig.19 It can be seen that the cycle performance and discharge capacity of the lithium-rich manganese-based composite positive electrode coated with lithium manganese iron phosphate in Example 8 are significantly improved compared with the uncoated comparative example 3 at a high temperature of 50°C.
[0123] In summary, the lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material of the present invention is mixed to uniformly wrap the lithium iron manganese phosphate on the surface of the lithium-rich manganese-based material, isolate the direct contact between the electrolyte and the lithium-rich manganese-based positive electrode material, and inhibit the occurrence of side reactions of the lithium-rich manganese-based positive electrode material. At the same time, the lithium generated by the phase change can enter the lithium iron manganese phosphate in the outer shell, reducing the loss of lithium and oxygen, not only retaining the high capacity of the lithium-rich manganese base itself, but also volatilizing the voltage stability and long cycle characteristics of the coating layer of the lithium iron manganese phosphate, so that the lithium-ion battery prepared by using the lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material has excellent voltage cycle and rate cycle performance.
[0124] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material, characterized in that: The lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material has a multilayer structure, which includes, from the inside to the outside, a lithium-rich manganese-based layer, a lithium iron manganese phosphate layer coated on the lithium-rich manganese-based layer, and a carbon layer outside the lithium iron manganese phosphate layer.
2. The lithium iron manganese phosphate coated lithium-rich manganese-based composite positive electrode material according to claim 1, characterized in that: The thickness of the lithium manganese iron phosphate layer and the carbon layer is 300-600 nm.
3. The method for preparing the lithium-rich manganese-based composite positive electrode material coated with lithium iron manganese phosphate according to claim 1, characterized in that: The following steps are involved: Step 1: uniformly mix the precursor and the lithium source at a molar ratio of 1:0.5-1.5, and heat at 1-10 °C min -1 The heating rate is firstly raised to 400-550°C in an air atmosphere in a muffle furnace and kept for 3-7h, then raised to 700-1000°C and kept for 5-20h, and then cooled naturally to obtain a lithium-rich manganese-based material with a molecular formula of Li[Li x Ni y Co z Mn k ]O2, where 0.07≤x≤0.26, 0 <y≤0.23,0<z≤0.17,0.43≤k≤0.68; Step 2, mix lithium manganese iron phosphate and a carbon source according to a mass ratio, and grind thoroughly to obtain a carbon-coated lithium manganese iron phosphate material, wherein the molecular formula of lithium manganese iron phosphate is LiMn a Fe b N c In PO4, 0 < a ≤ 0.6, 0 < b ≤ 1, 0 < c ≤ 0.6, and N is one or a combination of more than one of Cr, Cu, Al, Nb, Ti, or Co; Step 3, mixing the carbon-coated lithium manganese iron phosphate and the lithium-rich manganese base according to a mass ratio and grinding them thoroughly to obtain a composite positive electrode material with a multi-layer structure; or after grinding, heating to 50-300° C. under gas protection and keeping the temperature for 0-10 hours to obtain a composite positive electrode material with a multi-layer structure.
4. The preparation method according to claim 3, characterized in that: The precursor described in Step 1 is Mn m Co n Ni g T s (OH)2 or Mn m Co n Ni g T s CO3, 0 < g ≤ 0.4, 0 < n ≤ 0.45, 0 < m ≤ 0.75, 0 ≤ s ≤ 0.2, T is one or more combinations of Mg, Al, Ca, V, Mo, Fe, Nb or Zr; the lithium source is one or a mixture of two of Li2CO3 or LiOH·H2O.
5. The preparation method according to claim 3, characterized in that: Step 1 also includes doping with metal oxides, and the lithium-rich manganese-based material has a molecular formula of Li[Li x Ni y Co z Mn k M d ]O2, M is a doping element, where 0.07≤x≤0.25, 0 <y≤0.22,0<z≤0.16,0.43≤k≤0.65,0<d≤0.05。 6. The preparation method according to claim 5, characterized in that: The doped metal oxide is a mixture of one or more of MgO, Al2O3, TiO2, ZrO2, Nb2O5, Fe2O3, ZnO, CaO, V2O5, MoO3, WO3 or CuO.
7. The preparation method according to claim 3, characterized in that: In step 2, the mass of the carbon source accounts for 1-10% of the total mass of the lithium manganese iron phosphate and the carbon source, the particle size of the lithium manganese iron phosphate is 300-600nm, and the carbon source is one or more combinations of amorphous carbon, hard carbon, graphene, carbon nanotubes, and polyvinyl pyrrolidone.
8. The preparation method according to claim 3, characterized in that: In step 3, the mass of the carbon-coated lithium manganese iron phosphate accounts for 2-98% of the total mass of the composite positive electrode material, the particle size of the lithium-rich manganese base is 2-20 μm, and the protective gas is nitrogen, oxygen or argon.
9. Use of a lithium iron manganese phosphate-coated lithium-rich manganese-based composite positive electrode material according to claim 1 in the preparation of lithium-ion batteries.
10. The use according to claim 9, characterized in that: The current of the lithium ion battery in the constant current (CC) stage is 0.1-10C; the constant voltage (CV) is 4.4-4.7V; and the current under the constant voltage (CV) is 0.1-0.5 times that under the constant current (CC).
Citation Information
Cited By
Lithium manganese iron phosphate-lithium-rich manganese-based positive electrode material as well as preparation method and application thereof
CN119742335A
Modified lithium-rich manganese-based material and preparation method therefor, and positive electrode sheet and secondary battery
WO2026123215A1