Preparation method of modified coating of lithium ion battery diaphragm

Through the combination technology of polydopamine and silica particles, the problem of low adhesion of the separator coating of lithium-ion batteries is solved, which improves adhesion and thermal stability and extends the cycle life of the battery.

CN118970361APending Publication Date: 2024-11-15NANTONG UNIV +1

Patent Information

Application Number
CN202411010522.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The separator coating of traditional lithium-ion batteries has low adhesion, easy to block holes, consume electrolytes, and the capacity continues to decline during the cycle.

Method used

Using the combined technology of polydopamine and silica particles, the Tris-dopamine hydrochloride solution is formed by the reaction of ethyl orthosilicate-acetone solution and dopamine hydrochloride aqueous solution. After stirring and soaking, the adhesion of the coating on the surface of the membrane is improved. and lyophilic.

Benefits of technology

The uniform recombination of the coating is achieved, the adhesion, thermal stability and puncture strength are improved, the cycle life of the lithium-ion battery is extended, and the impact of lithium-ion conductivity is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970361A_ABST
    Figure CN118970361A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a lithium ion battery diaphragm modified coating, the modified coating is composed of polydopamine and silicon dioxide particles, and the preparation method comprises the following specific steps: mixing tetraethoxysilane and acetone, adding a dopamine hydrochloride solution while stirring, immersing a lithium ion battery diaphragm into the solution for reaction, filtering, washing, and drying to obtain the lithium ion battery diaphragm modified coating. And cleaning and drying to obtain the modified coating of the lithium ion battery diaphragm. The adhesive force of the coating is improved through dopamine auto-polymerization, the thermal stability of the diaphragm is enhanced through silicon dioxide particles, a porous structure is obtained based on the phase separation principle, the problem of hole blocking of a traditional coating is solved, and the method is simple and suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new energy materials, and specifically relates to a method for preparing a lithium-ion battery diaphragm modified coating. Background Art

[0002] The separator is a porous film sandwiched between the positive and negative electrodes of the battery, designed to prevent direct contact between the positive and negative electrodes while allowing ion transfer. Although the separator is an inactive component of the battery, its porosity, pore size, mechanical strength, thermal stability, hydrophilicity and other properties affect key performance such as ion transfer, cycle life, and safety. In lithium-ion power plants, repeated charge / discharge processes cause lithium dendrites to grow and pierce the separator, resulting in physical contact between the electrodes and internal short circuits. In addition, the large amount of heat generated during the charge / discharge process can also cause thermal shrinkage or even melting of the polymer separator, causing internal short circuits and battery failure. In extreme cases, these failures can also cause fires or explosions. In addition, in order to achieve rapid ion transfer, the separator needs to have a large porosity and good wettability with the electrolyte. Therefore, the development of high-performance separators with high thermal stability, high porosity and good electrolyte affinity is the key to the development of lithium-ion batteries with high energy density and long cycle life.

[0003] Silica coating can significantly improve the thermal stability and wettability of polyolefin separators. However, since a single silica coating is not easy to adhere to the surface of the separator and may lead to reduced porosity and consumption of electrolytes, its practical application is limited. Polydopamine presents a dense continuous film state on the surface of the substrate material. It can adhere to the surface of a variety of substrate materials (including precious metals, metal oxides, inorganic and polymer materials, etc.) and has almost no selectivity for the substrate. In addition, since the polydopamine coating contains a large number of catechol / benzoquinone groups that can participate in the reaction, the polydopamine coating has the possibility of secondary reaction with other substances.

[0004] The paper 10.1002 / anie.201915440 introduces a preparation method and application of a nano-scale silica coating directly attached to the surface of a polyolefin separator. The nano-shield protective separator can effectively inhibit the growth of lithium dendrites, and can reduce the stress intensity through the curved surface effect and form narrow channels to increase the growth path of lithium dendrites to alleviate the short circuit phenomenon and reduce the risk of battery spontaneous combustion or explosion. This method based on separator modification is compatible with the modification of electrodes / electrolytes, showing great potential for the development of high-energy density storage systems. However, the adhesion of the silica coating directly attached to the separator surface is relatively low and is not suitable for industrial applications.

[0005] The paper 10.1021 / am506797d introduces the use of a simple solution dip coating method to coat silica nanoparticles with large-scale pore structure on PE separators to obtain composite PE separators with better charge and discharge performance, cycle performance and dimensional stability. 2 Lithium-ion batteries with Nd / PE separators will cause a continuous decrease in capacity during the cycle process (the capacity decays by 18% after 100 cycles). Summary of the invention

[0006] Technical issues solved:

[0007] The present application aims to solve the technical problems that traditional coating modified coating has low adhesion on the surface of the diaphragm, is prone to pore clogging, consumes electrolyte, and continuously decreases capacity during the cycle, and provides a method for preparing a lithium-ion battery diaphragm modified coating composed of polydopamine and silica particles.

[0008] Technical solution:

[0009] To achieve the above objectives, this application is implemented through the following technical solutions:

[0010] A method for preparing a lithium-ion battery separator modified coating, the method comprising the following steps:

[0011] Step 1, respectively measuring ethyl orthosilicate and acetone in a volume ratio of ethyl orthosilicate:acetone=1:20-1:100 to prepare an ethyl orthosilicate-acetone solution;

[0012] Step 2, preparing a 1-5 g / L dopamine hydrochloride aqueous solution, adding tris(hydroxymethyl)aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution;

[0013] Step 3, under stirring, add the ethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 5 to 30 minutes;

[0014] Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone respectively;

[0015] Step 5, soaking the lithium-ion battery separator obtained in step 4 in the solution prepared in step 3 for 12 to 48 hours;

[0016] Step 6, taking out the lithium-ion battery separator obtained in step 5, and washing it with acetone and deionized water in turn;

[0017] Step 7: vacuum-dry the lithium-ion battery separator obtained in step 6.

[0018] Furthermore, in the step 1, the method for preparing the ethyl orthosilicate-acetone solution from ethyl orthosilicate and acetone is to measure ethyl orthosilicate and acetone respectively in a volume ratio of 1:20 to 1:100, and add ethyl orthosilicate dropwise into acetone while stirring to prepare the ethyl orthosilicate-acetone solution.

[0019] Furthermore, the preparation method of the 1-5 g / L dopamine hydrochloride aqueous solution in step 2 is to add dopamine hydrochloride particles to deionized water, slowly stir at 100 r / min to prepare 1-5 g / L dopamine hydrochloride aqueous solution, add tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5 to obtain a Tris-dopamine hydrochloride solution.

[0020] Furthermore, in step 3, the pH of Tris-dopamine hydrochloride is 8.5, the reaction time is 5 to 30 minutes, and the rotation speed is 500 r / min.

[0021] Furthermore, in step 4, the number of times of cleaning with deionized water and acetone is 3 times.

[0022] Furthermore, in step 6, the number of cleaning with deionized water and acetone is 3 times.

[0023] Furthermore, in step 7, the vacuum drying temperature is 30 to 80° C. and the drying time is 6 to 12 hours.

[0024] Beneficial effects:

[0025] The present application provides a method for preparing a modified coating of a lithium-ion battery separator, which has the following beneficial effects compared with the prior art:

[0026] 1. This application realizes the uniform compounding of the two at the molecular level through the self-polymerization of polydopamine and the in-situ hybridization modification technology of silica, improves the adhesion, thermal stability and lyophilicity of the coating on the surface of the polyolefin separator, the puncture strength is greater than 50g / um, the melting temperature is greater than 185°C, the thermal shrinkage rate at 130°C is less than 2%, and the contact angle is reduced from 104° to 30.9°;

[0027] 2. This application preferably uses highly volatile acetone as a solvent, and constructs a porous structure on the surface of the lithium-ion battery by a phase separation method, thereby reducing the effect of the polymer coating on the porosity and ionic conductivity of the diaphragm and increasing the ionic conductivity of the diaphragm to 10 -2 S cm -1 , extending the cycle life of lithium-ion batteries;

[0028] 3. The method provided by the present invention is easy to operate and can be easily industrialized on a large scale to modify lithium-ion battery separators. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is the water contact angle of the lithium ion battery separator before and after modification, wherein (a) is the water contact angle of the lithium ion battery separator before modification, and (b) is the water contact angle of the lithium ion battery separator after modification;

[0030] Figure 2 These are SEM images of the lithium-ion battery separator before and after modification, where (a) is the SEM image of the lithium-ion battery separator before modification, and (b) is the SEM image of the lithium-ion battery separator after modification. DETAILED DESCRIPTION

[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific embodiments of the present invention are described in detail below. Specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.

[0032] Embodiment 1:

[0033] A method for preparing a lithium-ion battery separator modified coating comprises the following steps:

[0034] Step 1, taking ethyl orthosilicate and acetone respectively in a volume ratio of ethyl orthosilicate: acetone = 1:30, and adding ethyl orthosilicate dropwise into acetone to prepare a ethyl orthosilicate-acetone solution;

[0035] Step 2, adding dopamine hydrochloride particles to deionized water, slowly stirring at 100 r / min to prepare a 1 g / L dopamine hydrochloride aqueous solution, adding tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution;

[0036] Step 3, under stirring, add the ethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 10 minutes at a speed of 500 r / min;

[0037] Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone three times respectively;

[0038] Step 5, soaking the lithium-ion battery separator obtained in step 4 in the solution prepared in step 3 for 24 hours;

[0039] Step 6, taking out the lithium-ion battery separator obtained in step 5, and washing it with acetone and deionized water three times in sequence;

[0040] Step 7: vacuum dry the lithium-ion battery separator obtained in step 6 at 50° C. for 8 h.

[0041] Embodiment 2:

[0042] A method for preparing a lithium-ion battery separator modified coating comprises the following steps:

[0043] Step 1, taking ethyl orthosilicate and acetone respectively in a volume ratio of ethyl orthosilicate: acetone = 1:40, and adding ethyl orthosilicate dropwise into acetone while stirring to prepare a ethyl orthosilicate-acetone solution;

[0044] Step 2, adding dopamine hydrochloride particles to deionized water, slowly stirring at 100 r / min to prepare a 2 g / L dopamine hydrochloride aqueous solution, adding tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution;

[0045] Step 3, under stirring, add the tetraethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 15 minutes at a speed of 500 r / min;

[0046] Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone three times respectively;

[0047] Step 5, soaking the lithium-ion battery separator obtained in step 4 in the solution prepared in step 3 for 24 hours;

[0048] Step 6, taking out the lithium-ion battery separator obtained in step 5, and washing it with acetone and deionized water three times in sequence;

[0049] Step 7: vacuum dry the lithium-ion battery separator obtained in step 6 at 40° C. for 11 hours.

[0050] Embodiment 3:

[0051] A method for preparing a lithium-ion battery separator modified coating comprises the following steps:

[0052] Step 1, taking ethyl orthosilicate and acetone respectively in a volume ratio of ethyl orthosilicate: acetone = 1:60, and adding ethyl orthosilicate dropwise into acetone while stirring to prepare a ethyl orthosilicate-acetone solution;

[0053] Step 2, adding dopamine hydrochloride particles to deionized water, slowly stirring at 100 r / min to prepare a 3 g / L dopamine hydrochloride aqueous solution, adding tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution;

[0054] Step 3, under stirring, add the tetraethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 20 minutes at a speed of 500 r / min;

[0055] Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone three times respectively;

[0056] Step 5, soaking the lithium ion battery separator obtained in step 4 in the solution prepared in step 3 for 36 hours;

[0057] Step 6, taking out the lithium-ion battery separator obtained in step 5, and washing it with acetone and deionized water three times in sequence;

[0058] Step 7: vacuum dry the lithium-ion battery separator obtained in step 6 at 60° C. for 10 hours.

[0059] Embodiment 4:

[0060] A method for preparing a lithium-ion battery separator modified coating comprises the following steps:

[0061] Step 1, taking ethyl orthosilicate and acetone respectively in a volume ratio of ethyl orthosilicate: acetone = 1:50, and adding ethyl orthosilicate dropwise into acetone while stirring to prepare a ethyl orthosilicate-acetone solution;

[0062] Step 2, adding dopamine hydrochloride particles to deionized water, slowly stirring at 100 r / min to prepare a 4 g / L dopamine hydrochloride aqueous solution, adding tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution;

[0063] Step 3, under stirring, add the tetraethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 25 minutes at a speed of 500 r / min;

[0064] Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone three times respectively;

[0065] Step 5, soaking the lithium-ion battery separator obtained in step 4 in the solution prepared in step 3 for 48 hours;

[0066] Step 6, after taking out the lithium-ion battery separator obtained in step 5, wash it with acetone and deionized water three times in sequence;

[0067] Step 7: vacuum dry the lithium-ion battery separator obtained in step 6 at 70° C. for 8 h.

[0068] Embodiment 5:

[0069] A method for preparing a lithium-ion battery separator modified coating comprises the following steps:

[0070] Step 1, taking ethyl orthosilicate and acetone respectively in a volume ratio of ethyl orthosilicate: acetone = 1:80, and adding ethyl orthosilicate dropwise into acetone while stirring to prepare a ethyl orthosilicate-acetone solution;

[0071] Step 2, adding dopamine hydrochloride particles to deionized water, slowly stirring at 100 r / min to prepare a 3 g / L dopamine hydrochloride aqueous solution, adding tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution;

[0072] Step 3, under stirring, add the tetraethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 25 minutes at a speed of 500 r / min;

[0073] Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone respectively;

[0074] Step 5, soaking the lithium-ion battery separator obtained in step 4 in the solution prepared in step 3 for 24 hours;

[0075] Step 6, after taking out the lithium-ion battery separator obtained in step 5, wash it with acetone and deionized water three times in sequence;

[0076] Step 7: vacuum dry the lithium-ion battery separator obtained in step 6 at 50° C. for 10 hours.

[0077] Embodiment 6:

[0078] A method for preparing a lithium-ion battery separator modified coating comprises the following steps:

[0079] Step 1, taking ethyl orthosilicate and acetone respectively in a volume ratio of ethyl orthosilicate: acetone = 1:100, and adding ethyl orthosilicate dropwise into acetone while stirring to prepare a ethyl orthosilicate-acetone solution;

[0080] Step 2, adding dopamine hydrochloride particles to deionized water, slowly stirring at 100 r / min to prepare a 5 g / L dopamine hydrochloride aqueous solution, adding tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution;

[0081] Step 3, under stirring, add the tetraethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 30 minutes at a speed of 500 r / min;

[0082] Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone three times respectively;

[0083] Step 5, soaking the lithium-ion battery separator obtained in step 4 in the solution prepared in step 3 for 48 hours;

[0084] Step 6, after taking out the lithium-ion battery separator obtained in step 5, wash it with acetone and deionized water three times in sequence;

[0085] Step 7: vacuum dry the lithium-ion battery separator obtained in step 6 at 30° C. for 12 h.

[0086] Embodiment 7:

[0087] A method for preparing a lithium-ion battery separator modified coating comprises the following steps:

[0088] Step 1, taking ethyl orthosilicate and acetone respectively in a volume ratio of ethyl orthosilicate: acetone = 3:100, and adding ethyl orthosilicate dropwise into acetone while stirring to prepare a ethyl orthosilicate-acetone solution;

[0089] Step 2, adding dopamine hydrochloride particles to deionized water, slowly stirring at 100 r / min to prepare a 1 g / L dopamine hydrochloride aqueous solution, adding tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution;

[0090] Step 3, under stirring, add the tetraethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 15 minutes at a speed of 500 r / min;

[0091] Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone three times respectively;

[0092] Step 5, soaking the lithium ion battery separator obtained in step 4 in the solution prepared in step 3 for 36 hours;

[0093] Step 6, after taking out the lithium-ion battery separator obtained in step 5, wash it with acetone and deionized water three times in sequence;

[0094] Step 7: vacuum dry the lithium-ion battery separator obtained in step 6 at 50° C. for 12 h.

[0095] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A method for preparing a lithium ion battery separator modified coating, characterized in that: The method comprises the following steps: Step 1, respectively measuring ethyl orthosilicate and acetone in a volume ratio of ethyl orthosilicate:acetone=1:20-1:100 to prepare an ethyl orthosilicate-acetone solution; Step 2, preparing a 1-5 g / L dopamine hydrochloride aqueous solution, adding tris(hydroxymethyl)aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5, to obtain a Tris-dopamine hydrochloride solution; Step 3, under stirring, add the ethyl orthosilicate-acetone solution prepared in step 1 dropwise into the Tris-dopamine hydrochloride with pH=8.5 prepared in step 2, and react for 5 to 30 minutes; Step 4, cleaning the surface of the lithium-ion battery separator with deionized water and acetone respectively; Step 5, soaking the lithium-ion battery separator obtained in step 4 in the solution prepared in step 3 for 12 to 48 hours; Step 6, taking out the lithium-ion battery separator obtained in step 5, and washing it with acetone and deionized water in turn; Step 7: vacuum drying the lithium-ion battery separator obtained in step 6.

2. The method for preparing a modified coating for a lithium ion battery separator according to claim 1, characterized in that: The method for preparing the ethyl orthosilicate-acetone solution from ethyl orthosilicate and acetone in step 1 is to measure ethyl orthosilicate and acetone respectively at a volume ratio of 1:20 to 1:100, and add ethyl orthosilicate dropwise into acetone while stirring to prepare the ethyl orthosilicate-acetone solution.

3. The method for preparing a modified coating for a lithium ion battery separator according to claim 1, characterized in that: The preparation method of the 1-5 g / L dopamine hydrochloride aqueous solution in step 2 is to add dopamine hydrochloride particles to deionized water, slowly stir at 100 r / min to prepare a 1-5 g / L dopamine hydrochloride aqueous solution, add tris (hydroxymethyl) aminomethane Tris particles to the dopamine hydrochloride aqueous solution to adjust the solution to a weakly alkaline pH of 8.5 to obtain a Tris-dopamine hydrochloride solution.

4. The method for preparing the modified coating of the lithium ion battery separator according to claim 1, characterized in that: In step 3, the pH of Tris-dopamine hydrochloride is 8.5, the reaction time is 5 to 30 minutes, and the rotation speed is 500 r / min.

5. The method for preparing a modified coating for a lithium ion battery separator according to claim 1, characterized in that: In step 4, the number of times of cleaning with deionized water and acetone is 3 times.

6. The method for preparing a modified coating for a lithium ion battery separator according to claim 1, characterized in that: In step 6, the number of times of cleaning with deionized water and acetone is 3 times.

7. The method for preparing the modified coating of the lithium ion battery separator according to claim 1, characterized in that: In step 7, the vacuum drying temperature is 30 to 80° C. and the drying time is 6 to 12 hours.

Citation Information

Patent Citations

  • Pretreatment method based on silica sol ceramic diaphragm

    CN103554549A

  • Preparation method for poly-dopamine modified ceramic particle nonwoven diaphragm

    CN105390642A

  • Method for preparing modified ceramic diaphragm through dopamine compound adhesive and application thereof

    CN106654125A

  • Microporous modified polypropylene lithium battery diaphragm and preparation method thereof

    CN113764827A

  • Preparation method of hydrophilic polypropylene material

    CN117468234A

Cited By

  • Diaphragm, battery and preparation method of diaphragm

    CN119725996A