Lithium metal battery diaphragm based on aramid nanofiber as well as preparation method and application of lithium metal battery diaphragm

Through the separator preparation method based on aramid nanofiber, the problem of dimensional shrinkage and transformation of lithium battery separators under high temperature conditions is solved, and a separator with high strength, high temperature resistance and safety is achieved, which significantly improves the cycle life and safety of the battery. .

CN118970363AInactive Publication Date: 2024-11-15SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202411034038.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium battery separators have dimensional shrinkage and transformation under high temperature conditions, resulting in lithium dendrites' growth and battery safety problems.

Method used

Using a separator preparation method based on aramid nanofibers, aramid nanofiber slurry is prepared by deprotonation treatment, and nanoinorganic ceramic particles and pore-forming agent are mixed, and nanoinorganic ceramic particles are dried by ultrasonic treatment and hot pressing to form nanoinorganic ceramic particles-aromatic Nanofiber composite separator improves the mechanical properties and lyophilicity of the separator.

Benefits of technology

Effectively inhibit the growth of lithium dendrites, prevent battery short circuit, improve cycle life and safety, ensure the dimensional stability of the separator under high temperature conditions, and significantly extend the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970363A_ABST
    Figure CN118970363A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium metal batteries, and discloses a lithium metal battery diaphragm based on aramid nanofiber as well as a preparation method and application thereof, and the preparation method comprises the following steps: carrying out deprotonation treatment on para-aramid fiber to prepare aramid nanofiber slurry; preparing ceramic slurry from the solid nano inorganic ceramic particles and N, N-dimethylacetamide; mixing the aramid nanofiber slurry with the ceramic slurry, adding a pore forming agent, and performing ultrasonic treatment to obtain aramid ceramic composite slurry; and blade-coating a preset substrate with the aramid fiber ceramic composite slurry, then carrying out solvent exchange with deionized water, and carrying out hot-pressing drying treatment to obtain the lithium metal battery diaphragm based on the aramid fiber nanofibers, the diaphragm prepared by the preparation method disclosed by the invention has super-strong mechanical properties, can effectively inhibit the growth of lithium dendrites in a circulating process, and prevents a battery short-circuit phenomenon caused by puncturing the diaphragm by the lithium dendrites, so that the safe use of the battery can be effectively ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries, and relates to the field of preparation of diaphragm materials for lithium metal batteries, and in particular to a lithium metal battery diaphragm based on aramid nanofibers, and a preparation method and application thereof. Background Art

[0002] Lithium metal has a high theoretical specific capacity (3860 mAh g -1 ), low density (0.534gcm -3 ) and the lowest electrochemical potential (-3.040V relative to the standard hydrogen electrode). The battery system with it as the negative electrode is widely used in all aspects of people's lives due to its advantages such as high conversion efficiency and fast response speed. It is considered to be an important research direction for the development of the entire battery industry. The diaphragm is an important component of the lithium battery. Its function is to prevent direct contact between the positive and negative electrodes, and at the same time enable ions to be freely transmitted in the electrolyte, which directly affects the battery's capacity, cycle and safety performance. Considering the needs of production, processing and manufacturing, the diaphragm should have properties such as selective permeability, high mechanical strength and corrosion resistance.

[0003] At present, commercial lithium battery separators are mainly polyolefin separators prepared by different stretching processes, but polyethylene or polypropylene separators have problems such as poor thermal stability, poor wettability to electrolyte, and insufficient strength. Specifically, generally speaking, the melting point of polyethylene is around 135°C, and its separator will show obvious dimensional shrinkage at high temperatures above 120°C. Therefore, how to inhibit the growth of lithium dendrites and prevent the occurrence of separator dimensional shrinkage has become a problem that the industry is currently trying to solve. Summary of the invention

[0004] In view of the technical problems existing in the prior art, the present invention provides a lithium metal battery separator based on aramid nanofibers and a preparation method and application thereof, so as to solve the technical problem of the separator size shrinkage and transformation phenomenon.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] The present invention provides a method for preparing a lithium metal battery separator based on aramid nanofibers, comprising:

[0007] Deprotonating the para-aramid fiber to prepare aramid nanofiber slurry;

[0008] A ceramic slurry is prepared by using solid nano inorganic ceramic particles and N,N-dimethylacetamide;

[0009] After mixing the aramid nanofiber slurry with the ceramic slurry, adding a pore-forming agent, and subjecting the mixture to ultrasonic treatment, an aramid ceramic composite slurry is obtained;

[0010] The aramid ceramic composite slurry is scraped onto a preset substrate, and then solvent exchange is performed with deionized water to obtain a gelled nano inorganic ceramic particle-aramid nano fiber composite diaphragm;

[0011] The gelled nano inorganic ceramic particle-aramid nanofiber composite diaphragm is subjected to hot pressing and drying treatment to obtain a nano inorganic ceramic particle-aramid nanofiber composite diaphragm, which is the aramid nanofiber-based lithium metal battery diaphragm.

[0012] Furthermore, the process of deprotonating the para-aramid fiber to prepare the aramid nanofiber slurry is as follows:

[0013] Para-aramid fiber, alkali, DMSO and methanol are mixed in a ratio of (1-1.5) g: (2-3) g: (145-150) mL: (3-5) mL, and magnetically stirred to obtain the aramid nanofiber slurry; wherein the alkali is potassium tert-butoxide or potassium hydroxide.

[0014] Furthermore, the mass ratio of the solid nano inorganic ceramic particles to the N,N-dimethylacetamide is (12-15):(80-90); wherein the solid nano inorganic ceramic particles are one of Al2O3, Si2O3, ZrO2 and 3Al2O3-2SiO2.

[0015] Furthermore, after the aramid nanofiber slurry is mixed with the ceramic slurry, a pore-forming agent is added, and ultrasonic treatment is performed to obtain an aramid ceramic composite slurry, the mass ratio of the aramid nanofiber slurry to the ceramic slurry is 3-5:1, and the pore-forming agent is dimethyl carbonate or polystyrene.

[0016] Furthermore, after the aramid nanofiber slurry is mixed with the ceramic slurry, a pore-forming agent is added, and the aramid ceramic composite slurry is obtained by ultrasonic treatment. The ultrasonic treatment temperature is 50-80° C. and the ultrasonic treatment time is 1-2 h.

[0017] Furthermore, the process of scraping the aramid ceramic composite slurry onto a preset substrate is specifically as follows: scraping the aramid ceramic composite slurry at a scraping amount of 20-30 g / m 2 Coated on glass substrate.

[0018] Furthermore, the process of performing solvent exchange with deionized water is specifically as follows: immersing the preset substrate coated with the aramid ceramic composite slurry in deionized water for 4-6 hours.

[0019] Furthermore, in the process of hot pressing and drying the gelled nano inorganic ceramic particles-aramid nano fiber composite membrane, the hot pressing and drying temperature is 70-80° C., the pressure is 5-8 MPa, and the time is 10-15 min.

[0020] The present invention also provides a lithium metal battery separator based on aramid nanofibers, which is prepared using the method for preparing the lithium metal battery separator based on aramid nanofibers.

[0021] The present invention also provides an application of a lithium metal battery separator based on aramid nanofibers, which is used for making a separator for a lithium metal battery.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The invention provides a method for preparing a lithium metal battery separator based on aramid nanofibers. The separator prepared by the method has super strong mechanical properties, can effectively inhibit the growth of lithium dendrites during the cycle process, and prevent the battery short circuit caused by the lithium dendrites piercing the separator, thereby effectively ensuring the safe use of the battery; at the same time, the cycle life is longer, and the prepared lithium-sulfur battery can be cycled for more than 500 cycles; specifically, the para-aramid fiber itself has excellent properties of flame retardancy, high temperature resistance, high modulus, high strength and insulation, and the size remains stable under high temperature conditions, which can significantly improve the service life and safety of the battery. ; By mixing nano-sized aramid fiber slurry with ceramic slurry, and then adding a reagent for adjusting the porosity and mixing them evenly through ultrasonic dispersion, the lyophilicity of the diaphragm material is improved after the introduction of nano-inorganic ceramic particles, thereby solving the problem that aramid fiber is difficult to wet in inorganic electrolytes; in addition, under the pore regulation effect of the pore-forming agent, the diaphragm has an appropriate pore size that can selectively pass lithium ions; compared with traditional film-forming technology, the adopted scraping method is easy to operate, simple and efficient, and can be suitable for large-scale continuous production of diaphragm materials, laying a theoretical foundation for its practical application in various fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 This is a flow chart of the preparation method of the aramid nanofiber-based lithium metal battery separator described in the present invention. DETAILED DESCRIPTION

[0026] In order to make the technical problems, technical solutions and beneficial effects solved by this application clearer, the technical solutions in the embodiments of this application will be described clearly and completely in combination with the drawings in the embodiments of this application; obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0027] As attached Figure 1 As shown, the present invention provides a method for preparing a lithium metal battery separator material based on aramid nanofibers, comprising the following steps:

[0028] Step 1: Deprotonate the para-aramid fiber to prepare aramid nanofiber slurry. The preparation process of the aramid nanofiber slurry is as follows:

[0029] In a wire-mouth bottle, para-aramid fiber, alkali, DMSO and methanol are added in sequence in a ratio of (1-1.5) g: (2-3) g: (145-150) mL: (3-5) mL, and magnetic stirring is performed for 48-72 h at a temperature of 70-80° C. and a rotation speed of 400-600 r / min to obtain a bright red viscose aramid nanofiber slurry, that is, the aramid nanofiber slurry is prepared; wherein the alkali is potassium tert-butoxide or potassium hydroxide, and the concentration of the aramid nanofiber slurry is 2wt%-3wt%.

[0030] Step 2: Prepare ceramic slurry using solid nano inorganic ceramic particles and N,N-dimethylacetamide. The preparation process of the ceramic slurry is as follows:

[0031] Weigh 12-15g of solid nano inorganic ceramic particles and 80-90g of DMAc, add the weighed solid nano inorganic ceramic particles and DMAc into a beaker and stir for 2-3h, then ultrasonically treat at 50-80°C for 2-10min to make them uniformly dispersed to obtain a ceramic slurry; wherein the solid nano inorganic ceramic particles include one of Al2O3, Si2O3, ZrO2 and 3Al2O3-2SiO2.

[0032] Step 3: After mixing the aramid nanofiber slurry with the ceramic slurry, add a pore-forming agent, and perform ultrasonic treatment to obtain an aramid ceramic composite slurry. The mass ratio of the aramid nanofiber slurry to the ceramic slurry is 3-5:1; the pore-forming agent is dimethyl carbonate or polystyrene; the ultrasonic treatment temperature is 50-80°C, and the ultrasonic treatment time is 1-2h.

[0033] Step 4: Scrape the aramid ceramic composite slurry onto a preset substrate, and then perform solvent exchange with deionized water to obtain a gelled nano-inorganic ceramic particle-aramid nano-fiber composite diaphragm.

[0034] Specifically, the aramid ceramic composite slurry is coated with a coating machine at a scraping amount of 20-30 g / m 2 Coated on a glass substrate, then soaked the glass substrate coated with the aramid ceramic composite slurry in deionized water for 4-6 hours for solvent exchange until the gel film on the glass substrate is completely gelled and automatically falls off.

[0035] Step 5: hot-press and dry the gelled nano inorganic ceramic particle-aramid nanofiber composite membrane to obtain a nano inorganic ceramic particle-aramid nanofiber composite membrane, which is the aramid nanofiber-based lithium metal battery membrane. Specifically, under the action of a vacuum pump of a paper sheet former, the gelled nano inorganic ceramic particle-aramid nanofiber composite membrane is hot-pressed and dried for 10-15 minutes at a hot-press drying temperature of 70-80°C and a pressure of 5-8MPa to obtain the nano inorganic ceramic particle-aramid nanofiber composite membrane.

[0036] The method for preparing the lithium metal battery separator described in the present invention can produce a separator with a tensile strength of up to 165 MPa. Compared with commonly used commercial separators such as polyethylene separators and polypropylene separators, the separator has superior mechanical properties, and can effectively inhibit the growth of lithium dendrites during the cycle process, preventing the battery short circuit caused by the puncture of the separator, thereby ensuring the safe use of the battery. At the same time, the cycle life is longer, and the prepared lithium-sulfur battery can be cycled for more than 500 times.

[0037] Preparation principle:

[0038] The preparation method of the lithium metal battery separator described in the present invention comprises mixing nano-sized aramid fiber slurry with ceramic slurry, adding a reagent for adjusting the porosity and mixing them evenly through ultrasonic dispersion, preparing a thin film material through a doctor blade method, and finally obtaining a nano-inorganic ceramic particle-aramid nano-fiber composite separator material with good thermal stability, high mechanical strength and good insulation after drying and forming.

[0039] Specifically, para-aramid nanofibers are used as the base material of the diaphragm, and the excellent properties of para-aramid fibers themselves, such as flame retardancy, high temperature resistance, high modulus, high strength and insulation, are utilized to ensure that the diaphragm maintains size stability under high temperature conditions while significantly improving the service life and safety of the battery; by introducing nano-inorganic ceramic particles, on the one hand, the aramid nanofibers themselves carry a negative charge and can adsorb the nano-inorganic ceramic particles through electrostatic action; on the other hand, the nano-aramid fibers are entangled and coiled, and the nano-inorganic ceramic particles interact with the aramid nanofibers through intermolecular hydrogen bonds to form a continuous porous network structure, thereby achieving the surface bonding of inorganic nanoparticles and aramid nanofibers. The surface is controllable and the contact angle between the composite diaphragm and the electrolyte is reduced as measured by an optical contact angle meter, which effectively improves the lyophilicity of the diaphragm material, thereby solving the problem that aramid fiber is difficult to wet in inorganic electrolytes. In addition, by adding dimethyl carbonate or polystyrene as a pore-forming agent, the pore-regulating effect of the pore-forming agent allows the diaphragm to have a pore size of appropriate size to selectively pass lithium ions. Secondly, the thin film material is prepared by the doctor blade coating method. Compared with the traditional film-forming technology, the doctor blade coating film-forming technology is easy to operate, simple and efficient, and can be suitable for the continuous production of large-scale diaphragm materials, laying a theoretical foundation for its practical application in various fields.

[0040] Example 1

[0041] This embodiment 1 provides a method for preparing a lithium metal battery separator based on aramid nanofibers, comprising the following steps:

[0042] Step 1: Add 1 g of PPTA fiber, 3 g of potassium tert-butoxide, 147 mL of DMSO and 3.6 mL of methanol to a wire bottle in sequence, and stir the mixture magnetically at 70° C. and 500 r / min for 48 h to obtain an aramid nanofiber slurry with a concentration of 2 wt%.

[0043] Step 2: Add 15 g of Al2O3 and 80 g of DMAc into a beaker and stir for 2 h, then perform ultrasonic treatment at 50°C for 2 min to uniformly disperse them to obtain a ceramic slurry.

[0044] Step 3: After mixing the aramid nanofiber slurry and the ceramic slurry in a mass ratio of 5:1, dimethyl carbonate is added, and ultrasonic treatment is performed at 50° C. for 1 h until the aramid nanofiber slurry is uniformly dispersed to obtain an aramid ceramic composite slurry.

[0045] Step 4: Use a coating machine to apply the aramid ceramic composite slurry at a scraping amount of 25 g / m 2The aramid ceramic composite slurry was coated on a glass substrate, and then the glass substrate coated with the aramid ceramic composite slurry was immersed in deionized water for 5 hours for solvent exchange until the gel film on the glass substrate was completely gelled and automatically fell off to obtain a gelled nano-inorganic ceramic particle-aramid nanofiber composite diaphragm.

[0046] Step 5. Under the action of the vacuum pump of the paper sheet former, the gelled nano-inorganic ceramic particles-aramid nanofiber composite membrane is hot-pressed and dried for 10 minutes at a hot-pressing drying temperature of 70°C and a pressure of 5 MPa to obtain an alumina-aramid nanofiber composite membrane, that is, the lithium metal battery membrane based on aramid nanofibers.

[0047] Performance testing:

[0048] The performance of the aramid nanofiber-based lithium metal battery separator prepared in this Example 1 was tested, and the test results were as follows: the tensile strength of the aramid nanofiber-based lithium metal battery separator was 160.8 MPa; after the aramid nanofiber-based lithium metal battery separator was placed in a 95°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were 0, and after being placed in a 105°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were <5%.

[0049] Example 2

[0050] This embodiment 2 provides a method for preparing a lithium metal battery separator based on aramid nanofibers, comprising the following steps:

[0051] Step 1: Add 1.5 g of PPTA fiber, 3 g of potassium tert-butoxide, 145 mL of DMSO and 3.6 mL of methanol into a wire bottle in sequence, stir the mixture magnetically at 70° C. and 400 r / min for 48 h to obtain an aramid nanofiber slurry with a concentration of 3 wt%.

[0052] Step 2: Add 15 g of Al2O3 and 85 g of DMAc into a beaker and stir for 2 h, then perform ultrasonic treatment at 60°C for 3 min to uniformly disperse them to obtain a ceramic slurry.

[0053] Step 3: After mixing the aramid nanofiber slurry and the ceramic slurry in a mass ratio of 5:1, dimethyl carbonate is added, and ultrasonic treatment is performed at 60° C. for 1 h until the aramid nanofiber slurry is uniformly dispersed to obtain an aramid ceramic composite slurry.

[0054] Step 4: Use a coating machine to apply the aramid ceramic composite slurry at a scraping amount of 20 g / m 2The aramid ceramic composite slurry was coated on a glass substrate, and then the glass substrate coated with the aramid ceramic composite slurry was immersed in deionized water for 4 hours for solvent exchange until the gel film on the glass substrate was completely gelled and automatically fell off to obtain a gelled nano-inorganic ceramic particle-aramid nanofiber composite diaphragm.

[0055] Step 5. Under the action of the vacuum pump of the paper sheet former, the gelled nano inorganic ceramic particles-aramid nanofiber composite membrane is hot-pressed and dried for 10 minutes at a hot-pressing drying temperature of 80°C and a pressure of 5 MPa to obtain an alumina-aramid nanofiber composite membrane, that is, the lithium metal battery membrane based on aramid nanofibers.

[0056] Performance testing:

[0057] The performance of the lithium metal battery separator based on aramid nanofibers prepared in this Example 2 was tested, and the test results were as follows: the tensile strength of the lithium metal battery separator based on aramid nanofibers was 148.3 MPa; after the lithium metal battery separator based on aramid nanofibers was placed in a 95°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were 0, and after being placed in a 105°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were <5%.

[0058] Example 3

[0059] This embodiment 3 provides a method for preparing a lithium metal battery separator based on aramid nanofibers, comprising the following steps:

[0060] Step 1: Add 1 g of PPTA fiber, 3 g of potassium hydroxide, 150 mL of DMSO and 3.6 mL of methanol to a wire bottle in sequence, stir the mixture magnetically at 70° C. and 600 r / min for 72 h to obtain an aramid nanofiber slurry with a concentration of 2 wt%.

[0061] Step 2: Add 15 g of SiO2 and 85 g of DMAc into a beaker and stir for 2 h, then perform ultrasonic treatment at 70 °C for 5 min to uniformly disperse them to obtain a ceramic slurry.

[0062] Step 3: After mixing the aramid nanofiber slurry and the ceramic slurry in a mass ratio of 3:1, polystyrene is added, and ultrasonic treatment is performed at 70° C. for 1 h until the aramid nanofiber slurry is evenly dispersed to obtain an aramid ceramic composite slurry.

[0063] Step 4: Use a coating machine to apply the aramid ceramic composite slurry at a scraping amount of 30 g / m 2The aramid ceramic composite slurry was coated on a glass substrate, and then the glass substrate coated with the aramid ceramic composite slurry was immersed in deionized water for 6 hours for solvent exchange until the gel film on the glass substrate was completely gelled and automatically fell off to obtain a gelled nano-inorganic ceramic particle-aramid nanofiber composite diaphragm.

[0064] Step 5. Under the action of the vacuum pump of the paper sheet former, the gelled nano-inorganic ceramic particles-aramid nanofiber composite membrane is hot-pressed and dried for 15 minutes at a hot-pressing drying temperature of 70°C and a pressure of 5 MPa to obtain a silica-aramid nanofiber composite membrane, that is, the lithium metal battery membrane based on aramid nanofibers is obtained.

[0065] Performance testing:

[0066] The performance of the lithium metal battery separator based on aramid nanofibers prepared in this Example 3 was tested, and the test results were as follows: the tensile strength of the lithium metal battery separator based on aramid nanofibers was 152.7 MPa; after the lithium metal battery separator based on aramid nanofibers was placed in a 95°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were 0, and after being placed in a 105°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were <5%.

[0067] Example 4

[0068] This embodiment 4 provides a method for preparing a lithium metal battery separator based on aramid nanofibers, comprising the following steps:

[0069] Step 1: Add 1.5 g of PPTA fiber, 3 g of potassium tert-butoxide, 147 mL of DMSO and 3 mL of methanol into a wire-mouth bottle in sequence, and stir the mixture magnetically at 70° C. and 500 r / min for 48 h to obtain an aramid nanofiber slurry with a concentration of 3 wt%.

[0070] Step 2: Add 15 g of ZrO2 and 90 g of DMAc into a beaker and stir for 2 h, then perform ultrasonic treatment at 50 °C for 10 min to uniformly disperse them to obtain a ceramic slurry.

[0071] Step 3: After mixing the aramid nanofiber slurry and the ceramic slurry in a mass ratio of 4:1, polystyrene is added, and ultrasonic treatment is performed at 50° C. for 2 h until the aramid nanofiber slurry is uniformly dispersed to obtain an aramid ceramic composite slurry.

[0072] Step 4: Use a coating machine to apply the aramid ceramic composite slurry at a scraping amount of 25 g / m 2The aramid ceramic composite slurry was coated on a glass substrate, and then the glass substrate coated with the aramid ceramic composite slurry was immersed in deionized water for 5 hours for solvent exchange until the gel film on the glass substrate was completely gelled and automatically fell off to obtain a gelled nano-inorganic ceramic particle-aramid nanofiber composite diaphragm.

[0073] Step 5. Under the action of the vacuum pump of the paper sheet former, the gelled nano-inorganic ceramic particles-aramid nanofiber composite membrane is hot-pressed and dried for 15 minutes at a hot-pressing drying temperature of 80°C and a pressure of 8MPa to obtain a zirconium oxide-aramid nanofiber composite membrane, that is, the lithium metal battery membrane based on aramid nanofibers is obtained.

[0074] Performance testing:

[0075] The performance of the aramid nanofiber-based lithium metal battery separator prepared in Example 4 was tested, and the test results were as follows: the tensile strength of the aramid nanofiber-based lithium metal battery separator was 144.6 MPa; after the aramid nanofiber-based lithium metal battery separator was placed in a 95°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were 0, and after being placed in a 105°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were <5%.

[0076] Example 5

[0077] This embodiment 5 provides a method for preparing a lithium metal battery separator based on aramid nanofibers, comprising the following steps:

[0078] Step 1: Add 1.5 g of PPTA fiber, 3 g of potassium hydroxide, 147 mL of DMSO and 4.5 mL of methanol into a wire bottle in sequence, stir the mixture magnetically at 70° C. and 500 r / min for 72 h to obtain an aramid nanofiber slurry with a concentration of 3 wt%.

[0079] Step 2: Add 15 g of 3Al2O3-2SiO2 and 90 g of DMAc into a beaker and stir for 2 h, then perform ultrasonic treatment at 50°C for 8 min to uniformly disperse the mixture to obtain a ceramic slurry.

[0080] Step 3: After mixing the aramid nanofiber slurry and the ceramic slurry in a mass ratio of 4.5:1, polystyrene is added, and ultrasonic treatment is performed at 50° C. for 2 h until the aramid nanofiber slurry is uniformly dispersed to obtain an aramid ceramic composite slurry.

[0081] Step 4: Use a coating machine to apply the aramid ceramic composite slurry at a scraping amount of 25 g / m 2The aramid ceramic composite slurry was coated on a glass substrate, and then the glass substrate coated with the aramid ceramic composite slurry was immersed in deionized water for 5 hours for solvent exchange until the gel film on the glass substrate was completely gelled and automatically fell off to obtain a gelled nano-inorganic ceramic particle-aramid nanofiber composite diaphragm.

[0082] Step 5. Under the action of the vacuum pump of the paper sheet former, the gelled nano inorganic ceramic particles-aramid nanofiber composite membrane is hot-pressed and dried for 10 minutes at a hot-pressing drying temperature of 80°C and a pressure of 8 MPa to obtain a mullite-aramid nanofiber composite membrane, that is, the lithium metal battery membrane based on aramid nanofibers.

[0083] Performance testing:

[0084] The performance of the aramid nanofiber-based lithium metal battery separator prepared in Example 5 was tested, and the test results were as follows: the tensile strength of the aramid nanofiber-based lithium metal battery separator was 147.6 MPa; after the aramid nanofiber-based lithium metal battery separator was placed in a 95°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were 0, and after being placed in a 105°C oven for 1 hour, its transverse and longitudinal heat shrinkage values ​​were <5%.

[0085] The method for preparing a lithium metal battery separator based on aramid nanofibers described in the present invention utilizes the inherent properties of aramid nanofiber membrane materials, such as high mechanical strength, good temperature resistance, and corrosion resistance, to ensure the safety requirements of lithium metal battery separators; at the same time, nano inorganic ceramic particles and pore-forming agents are introduced to regulate the porosity and lyophilicity of the separator; nano-sized aramid fiber slurry is mixed with ceramic slurry, and then a reagent for adjusting the porosity is added and mixed evenly through ultrasonic dispersion, and a thin film material is prepared by a doctor blade method, and after drying and molding, a separator material with good thermal stability, high mechanical strength, and good insulation is finally obtained.

[0086] The above embodiment is only one of the implementation methods that can realize the technical solution of the present invention. The scope of protection claimed by the present invention is not limited only to this embodiment, but also includes changes, replacements and other implementation methods that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention.

Claims

1. A method for preparing a lithium metal battery separator based on aramid nanofibers, characterized in that: include: Deprotonating the para-aramid fiber to prepare aramid nanofiber slurry; A ceramic slurry is prepared by using solid nano inorganic ceramic particles and N,N-dimethylacetamide; After mixing the aramid nanofiber slurry with the ceramic slurry, adding a pore-forming agent, and subjecting the mixture to ultrasonic treatment, an aramid ceramic composite slurry is obtained; The aramid ceramic composite slurry is scraped onto a preset substrate, and then solvent exchange is performed with deionized water to obtain a gelled nano inorganic ceramic particle-aramid nano fiber composite diaphragm; The gelled nano inorganic ceramic particle-aramid nanofiber composite diaphragm is subjected to hot pressing and drying treatment to obtain a nano inorganic ceramic particle-aramid nanofiber composite diaphragm, which is the aramid nanofiber-based lithium metal battery diaphragm.

2. The method for preparing a lithium metal battery separator based on aramid nanofibers according to claim 1, characterized in that: The process of deprotonating the para-aramid fiber to prepare the aramid nanofiber slurry is as follows: Para-aramid fiber, alkali, DMSO and methanol are mixed in a ratio of (1-1.5) g: (2-3) g: (145-150) mL: (3-5) mL, and magnetically stirred to obtain the aramid nanofiber slurry; wherein the alkali is potassium tert-butoxide or potassium hydroxide.

3. The method for preparing a lithium metal battery separator based on aramid nanofibers according to claim 1, characterized in that: The mass ratio of the solid nano inorganic ceramic particles to the N,N-dimethylacetamide is (12-15):(80-90); wherein the solid nano inorganic ceramic particles are one of Al2O3, Si2O3, ZrO2 and 3Al2O3-2SiO2.

4. The method for preparing a lithium metal battery separator based on aramid nanofibers according to claim 1, characterized in that: In the process of mixing the aramid nanofiber slurry with the ceramic slurry, adding a pore-forming agent, and subjecting the mixture to ultrasonic treatment to obtain an aramid ceramic composite slurry, the mass ratio of the aramid nanofiber slurry to the ceramic slurry is 3-5:1, and the pore-forming agent is dimethyl carbonate or polystyrene.

5. The method for preparing a lithium metal battery separator based on aramid nanofibers according to claim 1, characterized in that: After the aramid nanofiber slurry is mixed with the ceramic slurry, a pore-forming agent is added, and the aramid ceramic composite slurry is obtained by ultrasonic treatment. The ultrasonic treatment temperature is 50-80° C. and the ultrasonic treatment time is 1-2 hours.

6. The method for preparing a lithium metal battery separator based on aramid nanofibers according to claim 1, characterized in that: The process of scraping the aramid ceramic composite slurry onto a preset substrate is specifically as follows: scraping the aramid ceramic composite slurry at a scraping amount of 20-30 g / m 2 Coated on glass substrate.

7. The method for preparing a lithium metal battery separator based on aramid nanofibers according to claim 1, characterized in that: The process of solvent exchange with deionized water is specifically as follows: immersing the preset substrate coated with the aramid ceramic composite slurry in deionized water for 4-6 hours.

8. The method for preparing a lithium metal battery separator based on aramid nanofibers according to claim 1, characterized in that: In the process of hot pressing and drying the gelled nano inorganic ceramic particle-aramid nano fiber composite membrane, the hot pressing and drying temperature is 70-80° C., the pressure is 5-8 MPa, and the time is 10-15 min.

9. A lithium metal battery separator based on aramid nanofibers, characterized in that: The lithium metal battery separator is prepared by the method for preparing the aramid nanofiber-based lithium metal battery separator as described in claims 1-8.

10. The use of a lithium metal battery separator based on aramid nanofibers as claimed in claim 9, characterized in that: Used to make separators for lithium metal batteries.

Citation Information

Patent Citations

  • Ceramic aramid fiber coated diaphragm for lithium ion battery and preparation method of coated diaphragm

    CN110444714A

  • Para-aramid nanofiber / inorganic nanoparticle composite coating reinforced polyolefin battery diaphragm and preparation method thereof

    CN113206345A

  • Preparation method of aramid nanofiber-based battery diaphragm with micro-nano porous structure regulated and controlled by pore-foaming agent

    CN113506950A

  • Ceramic particle pore-forming aramid fiber coated lithium ion battery composite diaphragm and preparation method thereof

    CN114614196A

  • Para-aramid dissolving system and application thereof, aramid diaphragm and preparation method thereof, and aramid ceramic composite diaphragm and preparation method thereof

    CN115663394A

Cited By

  • Ultrathin quasi-solid electrolyte membrane, preparation method thereof and lithium metal battery

    CN120727970A

  • Aromatic polyamide separator for lithium batteries and method for its preparation

    CN122739719A