Vertical cavity surface emitting laser and preparation method thereof

By using a combination of Ge substrate and defect suppression layer, the problems of warpage and high stress in VCSELs on GaAs substrates were solved, resulting in a more uniform and thinner vertical cavity surface emission laser.

CN118970626APending Publication Date: 2024-11-15YANGZHOU CHANGELIGHT
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411166767.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The growth of epitaxial layers on GaAs substrates in existing vertical cavity surface-emitting lasers (VCSELs) can easily lead to wafer warping, affecting device uniformity, and the large thickness of the DBR reflective layer results in greater stress.

Method used

A Ge substrate is used instead of a GaAs substrate, and a defect suppression layer is set between the N-type Ge substrate and the N-type DBR reflective layer. AlGaInP, AlInP, or GaInP layers are used to suppress anti-phase domain defects, and the lattice matching of Ge materials is combined to reduce stress and warping.

Benefits of technology

By lattice matching between the Ge substrate and the N-type DBR reflective layer, the generation of reverse domain defects can be reduced or avoided, improving device uniformity. Furthermore, the epitaxial structure can be separated by etching to achieve a thinner VCSEL.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970626A_ABST
    Figure CN118970626A_ABST
Patent Text Reader

Abstract

The invention discloses a vertical-cavity surface-emitting laser and a preparation method thereof, and relates to the technical field of photoelectric devices, the vertical-cavity surface-emitting laser does not use a GaAs substrate, but uses a Ge substrate, and an N-type DBR reflecting layer, a first limiting layer, an active layer, a second limiting layer, an oxidation limiting layer and a P-type DBR reflecting layer are stacked on one side of the N-type Ge substrate. The N-type DBR reflecting layer comprises an Al < x > GaAs layer and an Al < y > GaAs layer, x < lt > which are alternately stacked; y. As the crystal lattice of the Ge material is larger than that of the GaAs material and is better matched with that of the AlGaAs material of the N-type DBR reflecting layer, stress and warping can be reduced by adopting the N-type Ge substrate, and the uniformity of the device is improved; the crystal orientation of the N-type Ge substrate is set to be larger than or equal to 2 degrees from a 100 plane to a 111 plane, and a defect suppression layer is arranged between the N-type Ge substrate and the N-type DBR reflecting layer to suppress anti-phase domain defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of optoelectronic devices, and in particular to a vertical cavity surface emitting laser and a method for preparing the same. Background Art

[0002] Vertical Cavity Surface Emitting Laser (VCSEL) is a semiconductor microcavity laser. Compared with traditional edge-emitting lasers, VCSELs have the advantages of low threshold current, small size, circularly symmetric spot for easy fiber coupling, high beam quality, single longitudinal mode, and easy integration of surface emission. They have been rapidly developed in recent years and are widely used in three-dimensional sensing, optical communications, lidar, unmanned driving and other fields such as face recognition.

[0003] The most mature and widely used VCSEL is the oxidation-limited VCSEL. Figure 1 As shown, it is mainly composed of an active layer, upper and lower limiting layers, upper and lower reflecting layers, an oxidized limiting layer, and upper and lower electrodes. Among them, the active layer is composed of multiple quantum wells; the upper and lower sides of the active layer are limiting layers, which play the role of limiting carriers and adjusting the cavity length; the upper and lower sides of the limiting layer are P-type DBR (Distributed Bragg Reflection) reflecting layer and N-type DBR reflecting layer, respectively. The P-type DBR reflecting layer and the N-type DBR reflecting layer are respectively formed by repeatedly stacking two materials with different refractive indices with a thickness of 1 / 4 optical wavelength. By adjusting the refractive index difference and logarithm of the two materials, the reflectivity can be as high as more than 99%; an oxidized limiting layer is arranged between the active layer and the P-type DBR reflecting layer, and the oxidized limiting layer is composed of a high-aluminum component material. After the wet selective oxidation process, the oxidized limiting layer forms an oxidized limiting window to achieve the limitation of current and light field; the P-type DBR reflecting layer and the N-type DBR reflecting layer are respectively metal ohmic contacts to form electrodes, and light windows are opened on the P side and the N side according to whether the device is a top emission structure or a bottom emission structure.

[0004] In order to obtain high reflectivity, the DBR reflective layer in the VCSEL requires, on the one hand, that the high refractive index layer and the low refractive index layer have a large refractive index difference, and on the other hand, that the high refractive index layer and the low refractive index layer have a large number of pairs. Taking the common 940nm VCSEL as an example, its DBR reflective layer requires about 50 pairs of high refractive index layers and low refractive index layers, totaling about 5μm-10μm. In this way, the thickness of the epitaxial layer will be thicker. Such a thick epitaxial layer grown on a GaAs substrate will have greater stress, which can easily cause wafer warping and affect device uniformity. Summary of the invention

[0005] To solve the above technical problems, the embodiments of the present application provide a vertical cavity surface emitting laser and a method for preparing the same, so as to utilize a Ge substrate instead of a GaAs substrate, so that the Ge substrate is more lattice-matched with the N-type DBR reflective layer, thereby reducing stress and warping and improving device uniformity.

[0006] To achieve the above objectives, the present application provides the following technical solutions:

[0007] A vertical cavity surface emitting laser, comprising:

[0008] An N-type Ge substrate, wherein the crystal orientation of the N-type Ge substrate is 100 plane and the deviation from 111 plane is greater than or equal to 2°;

[0009] A defect suppression layer located on one side of the N-type Ge substrate, wherein the defect suppression layer is an AlGaInP layer, an AlInP layer or a GaInP layer;

[0010] The defect suppression layer is located on the side away from the N-type Ge substrate, and the N-type DBR reflection layer, the first restriction layer, the active layer, the second restriction layer, the oxidation restriction layer and the P-type DBR reflection layer are stacked in a direction away from the N-type Ge substrate; the N-type DBR reflection layer includes a first refractive index layer and a second refractive index layer stacked alternately, and the first refractive index layer is Al x GaAs layer, the second refractive index layer is Al y GaAs layer, x <y。

[0011] Optionally, the In component of the defect suppression layer is in the range of 0.5%-0.7%, including endpoint values.

[0012] Optionally, the defect suppression layer is an AlGaInP layer or an AlInP layer, and an Al component of the defect suppression layer is greater than 20%.

[0013] Optionally, the defect suppression layer has a thickness ranging from 5 nm to 200 nm, including endpoint values.

[0014] Optionally, the defect suppression layer is doped with a surfactant, and the material of the surfactant is Sb material or Te material.

[0015] A method for preparing a vertical cavity surface emitting laser, comprising:

[0016] Providing an N-type Ge substrate, wherein the crystal orientation of the N-type Ge substrate is 100 plane and the deviation from 111 plane is greater than or equal to 2°;

[0017] forming a defect suppression layer on one side of the N-type Ge substrate, wherein the defect suppression layer is an AlGaInP layer, an AlInP layer or a GaInP layer, and the growth temperature range of the defect suppression layer is 650° C.-700° C., including end points;

[0018] On the side of the defect suppression layer away from the N-type Ge substrate, a stacked N-type DBR reflective layer, a first confinement layer, an active layer, a second confinement layer, an oxidation confinement layer, and a P-type DBR reflective layer are formed in a direction away from the N-type Ge substrate; the N-type DBR reflective layer includes alternately stacked first refractive index layers and second refractive index layers, and the first refractive index layer is Al x GaAs layer, and the second refractive index layer is Al y GaAs layer, where x < y.

[0019] Optionally, the In component range of the defect suppression layer is 0.5% - 0.7%, including the end values.

[0020] Optionally, the defect suppression layer is an AlGaInP layer or an AlInP layer, and the Al component of the defect suppression layer is greater than 20%.

[0021] Optionally, the thickness range of the defect suppression layer is 5 nm - 200 nm, including the end values.

[0022] Optionally, when forming the defect suppression layer, a surfactant is doped into the defect suppression layer, and the material of the surfactant is Sb material or Te material.

[0023] Compared with the prior art, the above technical solution has the following advantages:

[0024] The vertical cavity surface emitting laser provided by the embodiment of the present application no longer uses a GaAs substrate, but uses a Ge substrate. An N-type DBR reflective layer, a first confinement layer, an active layer, a second confinement layer, an oxidation confinement layer, and a P-type DBR reflective layer are stacked on one side of the N-type Ge substrate in a direction away from the N-type Ge substrate; among them, the first confinement layer, the active layer, the second confinement layer, and the oxidation confinement layer form a resonant cavity layer; the N-type DBR reflective layer includes alternately stacked first refractive index layers and second refractive index layers, the first refractive index layer is Al x GaAs layer, and the second refractive index layer is Al y GaAs layer, where x < y, that is, the first refractive index layer is a high refractive index layer with a low Al component, and the second refractive index layer is a low refractive index layer with a high Al component. Since the lattice of the Ge material is larger than that of the GaAs material and is closer to the AlAs lattice, and is more lattice-matched with the AlGaAs material of the N-type DBR reflective layer, therefore, using an N-type Ge substrate can reduce stress and warpage and improve device uniformity.

[0025] However, Ge material is a non-polar material, and AlGaAs material constituting the N-type DBR reflective layer is a polar material. When the N-type DBR reflective layer of AlGaAs material is grown on an N-type Ge substrate, an anti-phase domain defect will be generated. Then, by setting the crystal orientation of the N-type Ge substrate to be 100 plane and deviating from the 111 plane by 2° or more, and setting a defect suppression layer between the N-type Ge substrate and the N-type DBR reflective layer, and the defect suppression layer is an AlGaInP layer, an AlInP layer or a GaInP layer, the anti-phase domain defect can be suppressed. In this way, while the stress and warping are reduced by using the better matching of the lattice of the Ge substrate and the AlGaAs material of the N-type DBR reflective layer, the uniformity of the device is improved, and the generation of anti-phase domain defects can be reduced or avoided.

[0026] Furthermore, the In component of the defect suppression layer (AlGaInP layer, AlInP layer or GaInP layer) can be set in the range of 0.5%-0.7%, including the end value, so as to control the defect suppression layer to have an appropriate negative mismatch with respect to the Ge substrate, thereby improving the suppression effect of reverse domain defects.

[0027] When the defect suppression layer is an AlGaInP layer or an AlInP layer, the Al component of the defect suppression layer can be set to be greater than 20%, thereby utilizing the fact that Al atoms have a stronger affinity than Ga atoms and P atoms, are more likely to form bonds and are less likely to form reverse domains, to improve the suppression effect of reverse domain defects.

[0028] Optionally, the thickness of the defect suppression layer may be set to a range of 5 nm to 200 nm, including end points, to avoid the formation of anti-phase domains due to the inability to well transition interface defects due to the thin thickness of the defect suppression layer, thereby improving the suppression effect of reverse domain defects.

[0029] Furthermore, when the defect suppression layer is an AlGaInP layer or an AlInP layer, the Ge material can be resistant to HCl corrosion, while the AlGaInP material and the AlInP material are easily corroded by HCl, so as to separate the Ge substrate and the VCSEL epitaxial structure on the Ge substrate (mainly GaAs-based materials), so as to remove the Ge substrate and make the VCSEL thinner, or further transfer the VCSEL epitaxial structure to other substrates (such as a heat sink), for example, to form a VCSEL with a bottom emission structure.

[0030] In addition, a surfactant may be doped into the defect suppression layer. The material of the surfactant may be Sb material or Te material to optimize the surface of the defect suppression layer and facilitate the subsequent formation of an N-type DBR reflective layer on the defect suppression layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 It is a schematic diagram of the cross-sectional structure of an existing vertical cavity surface emitting laser;

[0033] Figure 2 A schematic cross-sectional structure diagram of a vertical cavity surface emitting laser provided in an embodiment of the present application;

[0034] Figure 3 A schematic flow chart of a method for preparing a vertical cavity surface emitting laser provided in an embodiment of the present application.

[0035] Reference numerals:

[0036] 10-N-type Ge substrate; 20-defect suppression layer; 30-N-type DBR reflection layer; 31-first refractive index layer; 32-second refractive index layer; 40-first confinement layer; 50-active layer; 51-barrier layer; 52-well layer; 60-second confinement layer; 70-oxidation confinement layer; 80-P-type DBR reflection layer; 81-third refractive index layer; 82-fourth refractive index layer; 90-buffer layer; 100-ohmic contact layer. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0038] In the following description, many specific details are set forth to facilitate a full understanding of the present application, but the present application may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.

[0039] Secondly, the present application is described in detail with reference to the schematic diagram. When describing the embodiments of the present application in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of the present application. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.

[0040] The present application embodiment provides a vertical cavity surface emitting laser, Figure 2 FIG. 4 shows a schematic cross-sectional structure diagram of a vertical cavity surface emitting laser provided in an embodiment of the present application. Figure 2 As shown, the vertical cavity surface emitting laser comprises:

[0041] An N-type Ge substrate 10, wherein the crystal orientation of the N-type Ge substrate 10 is 100 plane and the inclination of the plane to the 111 plane is greater than or equal to 2°;

[0042] A defect suppression layer 20 located on one side of the N-type Ge substrate 10, wherein the defect suppression layer 20 is an AlGaInP layer, an AlInP layer or a GaInP layer;

[0043] The N-type DBR reflective layer 30, the first restriction layer 40, the active layer 50, the second restriction layer 60, the oxidized restriction layer 70 and the P-type DBR reflective layer 80 are stacked in a direction away from the N-type Ge substrate 10 and located on the side of the defect suppression layer 20 away from the N-type Ge substrate 10; wherein the N-type DBR reflective layer 30 includes a first refractive index layer 31 and a second refractive index layer 32 stacked alternately, and the first refractive index layer 31 is Al x GaAs layer, the second refractive index layer 32 is Al y GaAs layer, x <y。

[0044] In the embodiment of the present application, the first confinement layer 40 , the active layer 50 , the second confinement layer 60 and the oxidized confinement layer 70 constitute a resonant cavity layer.

[0045] The active layer 50 includes barrier layers 51 and well layers 52 that are alternately stacked. The barrier layers 51 may be Al z1 The Al component of the GaInP layer can satisfy: 0.1≤z1≤0.4, and its thickness can be 5nm-10nm, including the end value. The barrier layer 51 can be doped with Sb, and the doping amount can be 1E18cm -3 -5E19 cm -3 , including endpoint values; the potential well layer 52 can be a GaInP layer, and its thickness can be 5nm-10nm, including endpoint values.

[0046] The first confinement layer 40 and the second confinement layer 60 may be Al z2 GaInP layer, in order to limit the overflow of carriers from the active layer 50, the Al component z2 of the first limiting layer 40 and the second limiting layer 60 is greater than or equal to the Al component z1 of the barrier layer 51 of the active layer 50, that is, z2 ≥ z1; the first limiting layer 40 and the second limiting layer 60 can be doped with Sb, and the doping amount can be 1E18 cm -3 -5E19 cm -3, including the endpoint values. In particular, the doping amount of Sb in the second confinement layer 60 is greater than that of Sb in the first confinement layer 40.

[0047] In the embodiment of the present application, the N-type DBR reflective layer 30 includes alternately stacked first refractive index layers 31 and second refractive index layers 32. The first refractive index layer 31 is an Al x GaAs layer, and the second refractive index layer 32 is an Al y GaAs layer, where x < y, that is, the first refractive index layer 31 is a high refractive index layer with a low Al component, and the second refractive index layer is a low refractive index layer with a high Al component. The number of periods of the first refractive index layer 31 and the second refractive index layer 32 is m pairs, where m is a positive integer. The optical thicknesses of both the first refractive index layer 31 and the second refractive index layer 32 are 1 / 4 optical wavelength. The N-type doping concentrations of the first refractive index layer 31 and the second refractive index layer 32 are the same, and can both be 2E18 cm -3 .

[0048] Similarly, the P-type DBR reflective layer 80 includes alternately stacked third refractive index layers 81 and fourth refractive index layers 82. The third refractive index layer 81 is an Al x1 GaAs layer, and the fourth refractive index layer 82 is an Al y1 GaAs layer, where x1 < y1, that is, the third refractive index layer 81 is a high refractive index layer with a low Al component, and the fourth refractive index layer 82 is a low refractive index layer with a high Al component. The number of periods of the third refractive index layer 81 and the fourth refractive index layer 82 is w pairs, where w is a positive integer. The optical thicknesses of both the third refractive index layer 81 and the fourth refractive index layer 82 are 1 / 4 optical wavelength.

[0049] In the vertical cavity surface emitting laser provided by the embodiment of the present application, a GaAs substrate is no longer used, but a Ge substrate is used. On one side of the N-type Ge substrate 10, the N-type DBR reflective layer 30, the first confinement layer 40, the active layer 50, the second confinement layer 60, the oxidation confinement layer 70, and the P-type DBR reflective layer 80 are stacked in a direction away from the N-type Ge substrate 10. The N-type DBR reflective layer 30 includes alternately stacked first refractive index layers 31 and second refractive index layers 32. The first refractive index layer 31 is an Al x GaAs layer, and the second refractive index layer 32 is an Al y GaAs layer, where x < y, that is, the first refractive index layer 31 is a high refractive index layer with a low Al component, and the second refractive index layer 32 is a low refractive index layer with a high Al component. Since the lattice of the Ge material is larger than that of the GaAs material and is closer to the AlAs lattice, it is more matched with the AlGaAs material lattice of the N-type DBR reflective layer. Therefore, using an N-type Ge substrate can reduce stress and warping and improve device uniformity.

[0050] However, Ge material is a non-polar material, and AlGaAs material constituting the N-type DBR reflective layer 30 is a polar material. When the N-type DBR reflective layer of AlGaAs material is grown on an N-type Ge substrate, anti-phase domain defects will be generated. Furthermore, by setting the crystal orientation of the N-type Ge substrate 10 to be 100 plane deviating from the 111 plane by 2° or more, and setting a defect suppression layer 20 between the N-type Ge substrate 10 and the N-type DBR reflective layer 30, and the defect suppression layer 20 is an AlGaInP layer, an AlInP layer or a GaInP layer, the anti-phase domain defects can be suppressed. In this way, while the AlGaAs material lattice of the Ge substrate and the N-type DBR reflective layer is more closely matched to reduce stress and warpage, and improve device uniformity, the generation of anti-phase domain defects can be reduced or avoided.

[0051] Further optionally, the In component of the defect suppression layer 20 (AlGaInP layer, AlInP layer or GaInP layer) can be set to a range of 0.5%-0.7%, including the endpoint values, so as to control the defect suppression layer 20 to have an appropriate negative mismatch relative to the N-type Ge substrate 10, thereby improving the suppression effect of reverse domain defects.

[0052] When the defect suppression layer 20 is an AlGaInP layer or an AlInP layer, the Al component of the defect suppression layer 20 can be set to be greater than 20%, thereby utilizing the characteristics that Al atoms have a stronger affinity than Ga atoms and P atoms, are more likely to form bonds and are less likely to form reverse domains, to improve the suppression effect of reverse domain defects.

[0053] Optionally, the thickness of the defect suppression layer 20 may be set to range from 5 nm to 200 nm, including end points, to avoid the formation of anti-phase domains due to the defect that the defect suppression layer 20 is too thin to well transition the interface defects, thereby improving the suppression effect of the reverse domain defects.

[0054] Furthermore, when the defect suppression layer 20 is an AlGaInP layer or an AlInP layer, the characteristics that the Ge material can resist corrosion by HCl, while the AlGaInP material and the AlInP material are easily corroded by HCl can be utilized to separate the N-type Ge substrate 10 and the VCSEL epitaxial structure on the N-type Ge substrate 10 (mainly GaAs-based materials, including the N-type DBR reflective layer 30, the first confinement layer 40, the active layer 50, the second confinement layer 60, the oxidation confinement layer 70 and the P-type DBR reflective layer 80), so as to facilitate the removal of the N-type Ge substrate 10, making the VCSEL thinner and lighter, or further transferring the VCSEL epitaxial structure to other substrates (such as a heat sink), for example, forming a VCSEL with a bottom emission structure.

[0055] Thus, the defect suppression layer 20 between the N-type Ge substrate 10 and the N-type DBR reflective layer 30 can not only suppress antiphase domain defects, but also serve as an etching sacrificial layer to separate the N-type Ge substrate 10 and the N-type DBR reflective layer 30 .

[0056] It should be noted that when the defect suppression layer 20 is a GaInP layer, a corrosion sacrificial layer (such as an AlInP layer) can also be set between the defect suppression layer 20 and the N-type DBR reflective layer 30, so that the defect suppression layer 20 can be used to suppress the anti-phase domain defects between the N-type Ge substrate 10 and the N-type DBR reflective layer 30, and the corrosion sacrificial layer is added to separate the N-type Ge substrate 10 and the N-type DBR reflective layer 30.

[0057] Based on any of the above embodiments, optionally, a surfactant may be doped into the defect suppression layer 20 , wherein the material of the surfactant is Sb material or Te material, so as to optimize the surface of the defect suppression layer 20 , thereby facilitating the subsequent formation of an N-type DBR reflective layer on the defect suppression layer 20 .

[0058] like Figure 2 As shown, the vertical cavity surface emitting laser provided in the embodiment of the present application may further include a buffer layer 90 located between the defect suppression layer 20 and the N-type DBR reflective layer 30 , and the buffer layer 90 may be a GaAs layer.

[0059] like Figure 2 As shown, the vertical cavity surface emitting laser provided in the embodiment of the present application may further include an ohmic contact layer 100 located on the side of the P-type DBR reflective layer 80 away from the N-type Ge substrate 10, so that the P-type DBR reflective layer 80 is electrically connected to the P electrode through the ohmic contact layer 100. In addition, a SiN layer or a SiO layer may be plated on the back of the N-type Ge substrate 10 to form an N electrode, so that the N electrode is electrically connected to the N-type DBR reflective layer 30 through the N-type Ge substrate 10.

[0060] The vertical cavity surface emitting laser provided in the embodiment of the present application can be a top emitting structure, that is, a light window is opened from the P surface, or a bottom emitting structure, that is, a light window is opened from the N surface.

[0061] Accordingly, the present invention also provides a method for preparing a vertical cavity surface emitting laser. Figure 3 A schematic diagram showing a process of preparing a vertical cavity surface emitting laser provided in an embodiment of the present application is shown, combined with Figure 2 and Figure 3 As shown, the preparation method of the vertical cavity surface emitting laser includes:

[0062] S10: providing an N-type Ge substrate 10, wherein the crystal orientation of the N-type Ge substrate 10 is 100 plane and the deviation from 111 plane is greater than or equal to 2°;

[0063] S20: Form a defect suppression layer 20 on one side of the N-type Ge substrate 10. The defect suppression layer 20 is an AlGaInP layer, an AlInP layer or a GaInP layer. The growth temperature range of the defect suppression layer 20 is 600°C - 700°C, including the endpoint values;

[0064] S30: On the side of the defect suppression layer 20 facing away from the N-type Ge substrate 10, form a stacked N-type DBR reflective layer 30, a first confinement layer 40, an active layer 50, a second confinement layer 60, an oxidation confinement layer 70 and a P-type DBR reflective layer 80 in the direction away from the N-type Ge substrate 10.

[0065] Among them, the N-type DBR reflective layer 30 includes alternately stacked first refractive index layers 31 and second refractive index layers 32. The first refractive index layer 31 is an Al x GaAs layer, and the second refractive index layer 32 is an Al y GaAs layer, where x < y, that is, the first refractive index layer 31 is a high refractive index layer with a low Al component, and the second refractive index layer is a low refractive index layer with a high Al component. The number of period pairs of the first refractive index layer 31 and the second refractive index layer 32 is m pairs, where m is a positive integer. The optical thicknesses of both the first refractive index layer 31 and the second refractive index layer 32 are 1 / 4 optical wavelength. The doping concentrations of the first refractive index layer 31 and the second refractive index layer 32 are the same, and can both be 2E18 cm -3 .

[0066] Similarly, the P-type DBR reflective layer 80 includes alternately stacked third refractive index layers 81 and fourth refractive index layers 82. The third refractive index layer 81 is an Al x1 GaAs layer, and the fourth refractive index layer 82 is an Al y1 GaAs layer, where x1 < y1, that is, the third refractive index layer 81 is a high refractive index layer with a low Al component, and the fourth refractive index layer 82 is a low refractive index layer with a high Al component. The number of period pairs of the third refractive index layer 81 and the fourth refractive index layer 82 is w pairs, where w is a positive integer. The optical thicknesses of both the third refractive index layer 81 and the fourth refractive index layer 82 are 1 / 4 optical wavelength.

[0067] In the embodiment of the present application, the first confinement layer 40, the active layer 50, the second confinement layer 60 and the oxidation confinement layer 70 constitute a resonant cavity layer.

[0068] Among them, the active layer 50 includes alternately stacked barrier layers 51 and well layers 52. The barrier layer 51 can be an Al z1 GaInP layer, and its Al component can satisfy: 0.1 ≤ z1 ≤ 0.4, and its thickness can be 5 nm - 10 nm, including the endpoint values. The barrier layer 51 can be doped with Sb, and the doping amount can be 1E18 cm -3 -5E19 cm -3, including the endpoint values; the potential well layer 52 can be a GaInP layer, and its thickness can be 5 nm - 10 nm, including the endpoint values.

[0069] The first confinement layer 40 and the second confinement layer 60 can be Al z2 GaInP layers. In order to limit the carrier overflow of the active layer 50, the Al composition z2 of the first confinement layer 40 and the second confinement layer 60 is greater than or equal to the Al composition z1 of the barrier layer 51 of the active layer 50, that is, z2 ≥ z1; the first confinement layer 40 and the second confinement layer 60 can be doped with Sb, and the doping amount can be 1E18 cm -3 -5E19 cm -3 , including the endpoint values. In particular, the doping amount of Sb in the second confinement layer 60 is greater than the doping amount of Sb in the first confinement layer 40.

[0070] The method for preparing the vertical cavity surface emitting laser provided by the embodiments of the present application no longer uses a GaAs substrate, but uses a Ge substrate. A stacked N-type DBR reflective layer 30, a first confinement layer 40, an active layer 50, a second confinement layer 60, an oxidation confinement layer 70, and a P-type DBR reflective layer 80 are formed on one side of the N-type Ge substrate 10 in a direction away from the N-type Ge substrate 10. The N-type DBR reflective layer 30 includes alternately stacked first refractive index layers 31 and second refractive index layers 32. The first refractive index layer 31 is an Al x GaAs layer, and the second refractive index layer 32 is an Al y GaAs layer, x < y, that is, the first refractive index layer 31 is a high refractive index layer with a low Al composition, and the second refractive index layer 32 is a low refractive index layer with a high Al composition. Since the lattice of the Ge material is larger than the lattice of the GaAs material and is closer to the AlAs lattice, it is more lattice-matched with the AlGaAs material of the N-type DBR reflective layer. Therefore, using an N-type Ge substrate can reduce stress and warping and improve device uniformity.

[0071] However, the Ge material is a non-polar material, and the AlGaAs material constituting the N-type DBR reflective layer 30 is a polar material. Growing an N-type DBR reflective layer of AlGaAs material on an N-type Ge substrate will generate antiphase domain defects. Furthermore, by setting the crystal orientation of the N-type Ge substrate 10 to be greater than or equal to 2° off the 111 plane from the 100 plane, and setting a defect suppression layer 20 between the N-type Ge substrate 10 and the N-type DBR reflective layer 30, and the defect suppression layer 20 is an AlGaInP layer, an AlInP layer, or a GaInP layer, and the growth temperature of the defect suppression layer 20 is controlled in the range of 650 °C - 700 °C, the antiphase domain defects are suppressed. In this way, while taking advantage of the better lattice matching between the Ge substrate and the AlGaAs material of the N-type DBR reflective layer to reduce stress and warping and improve device uniformity, the generation of reverse domain defects can be reduced or avoided.

[0072] It should be noted that the growth temperature of the defect suppression layer 20 is controlled in the range of 650°C-700°C, that is, the growth temperature of the defect suppression layer 20 is moderately high, thereby improving the atomic migration ability, so that the Ga atoms and other group III atoms in the defect suppression layer 20 have a certain kinetic energy, so that they are more able to move to suitable sites to form bonds, rather than forming reverse domain defects, so as to reduce or avoid the generation of reverse domain defects.

[0073] Further optionally, the In component of the defect suppression layer 20 (AlGaInP layer, AlInP layer or GaInP layer) can be set to a range of 0.5%-0.7%, including the endpoint values, so as to control the defect suppression layer 20 to have an appropriate negative mismatch relative to the N-type Ge substrate 10, thereby improving the suppression effect of reverse domain defects.

[0074] When the defect suppression layer 20 is an AlGaInP layer or an AlInP layer, the Al component of the defect suppression layer 20 can be set to be greater than 20%, thereby utilizing the characteristics that Al atoms have a stronger affinity than Ga atoms and P atoms, are more likely to form bonds and are less likely to form reverse domains, to improve the suppression effect of reverse domain defects.

[0075] Optionally, the thickness of the defect suppression layer 20 may be set to range from 5 nm to 200 nm, including end points, to avoid the formation of anti-phase domains due to the defect that the defect suppression layer 20 is too thin to well transition the interface defects, thereby improving the suppression effect of the reverse domain defects.

[0076] Furthermore, when the defect suppression layer 20 is an AlGaInP layer or an AlInP layer, the characteristics that the Ge material can resist corrosion by HCl, while the AlGaInP material and the AlInP material are easily corroded by HCl can be utilized to separate the N-type Ge substrate 10 and the VCSEL epitaxial structure on the N-type Ge substrate 10 (mainly GaAs-based materials, including the N-type DBR reflective layer 30, the first confinement layer 40, the active layer 50, the second confinement layer 60, the oxidation confinement layer 70 and the P-type DBR reflective layer 80), so as to facilitate the removal of the N-type Ge substrate 10, making the VCSEL thinner and lighter, or further transferring the VCSEL epitaxial structure to other substrates (such as a heat sink), for example, forming a VCSEL with a bottom emission structure.

[0077] Thus, the defect suppression layer 20 between the N-type Ge substrate 10 and the N-type DBR reflective layer 30 can not only suppress antiphase domain defects, but also serve as an etching sacrificial layer to separate the N-type Ge substrate 10 and the N-type DBR reflective layer 30 .

[0078] It should be noted that when the defect suppression layer 20 is a GaInP layer, a corrosion sacrificial layer (such as an AlInP layer) can also be set between the defect suppression layer 20 and the N-type DBR reflective layer 30, so that the defect suppression layer 20 can be used to suppress the anti-phase domain defects between the N-type Ge substrate 10 and the N-type DBR reflective layer 30, and the corrosion sacrificial layer is added to separate the N-type Ge substrate 10 and the N-type DBR reflective layer 30.

[0079] Based on any of the above embodiments, optionally, when forming the defect suppression layer 20, a surfactant may be doped into the defect suppression layer 20, and the material of the surfactant is Sb material or Te material, so as to optimize the surface of the defect suppression layer 20, so as to facilitate the subsequent formation of an N-type DBR reflective layer on the defect suppression layer 20.

[0080] like Figure 1 As shown, before forming the N-type DBR reflective layer 30, the method for preparing the vertical cavity surface emitting laser provided in the embodiment of the present application may further include:

[0081] S40 : forming a buffer layer 90 on the side of the defect suppression layer 20 away from the N-type Ge substrate 10 . The buffer layer 90 may be a GaAs layer.

[0082] Subsequently, an N-type DBR reflective layer 30 is formed on the side of the buffer layer 90 away from the N-type Ge substrate 10 .

[0083] like Figure 1 As shown, after forming the P-type DBR reflective layer 80, the method for preparing the vertical cavity surface emitting laser provided in the embodiment of the present application may further include:

[0084] S50 : forming an ohmic contact layer 100 on the side of the P-type DBR reflective layer 80 away from the N-type Ge substrate 10 , so that the P-type DBR reflective layer 80 is subsequently electrically connected to the P electrode through the ohmic contact layer 100 .

[0085] In addition, a SiN layer or a SiO layer may be plated on the back of the N-type Ge substrate 10 to form an N-electrode, so that the N-electrode is electrically connected to the N-type DBR reflective layer 30 through the N-type Ge substrate 10 .

[0086] The vertical cavity surface emitting laser prepared by the method provided in the embodiment of the present application can be a top emitting structure, that is, a light window is opened from the P surface, or a bottom emitting structure, that is, a light window is opened from the N surface.

[0087] In summary, the vertical cavity surface emitting laser and its manufacturing method provided by the embodiments of the present application no longer use a GaAs substrate, but use a Ge substrate. On one side of the N-type Ge substrate 10, an N-type DBR reflective layer 30, a first confinement layer 40, an active layer 50, a second confinement layer 60, an oxidation confinement layer 70, and a P-type DBR reflective layer 80 are stacked in a direction away from the N-type Ge substrate 10. The N-type DBR reflective layer 30 includes alternately stacked first refractive index layers 31 and second refractive index layers 32. The first refractive index layer 31 is an Al x GaAs layer, and the second refractive index layer 32 is an Al y GaAs layer, where x < y, that is, the first refractive index layer 31 is a high refractive index layer with a low Al component, and the second refractive index layer 32 is a low refractive index layer with a high Al component. Since the lattice of the Ge material is larger than that of the GaAs material and is closer to the AlAs lattice, it is more lattice-matched with the AlGaAs material of the N-type DBR reflective layer. Therefore, using an N-type Ge substrate can reduce stress and warping and improve device uniformity.

[0088] However, the Ge material is a non-polar material, and the AlGaAs material constituting the N-type DBR reflective layer 30 is a polar material. Growing an N-type DBR reflective layer of AlGaAs material on an N-type Ge substrate will generate antiphase domain defects. Furthermore, by setting the crystal orientation of the N-type Ge substrate 10 to be greater than or equal to 2° away from the 111 plane with respect to the 100 plane, and providing a defect suppression layer 20 between the N-type Ge substrate 10 and the N-type DBR reflective layer 30, and the defect suppression layer 20 is an AlGaInP layer, an AlInP layer, or a GaInP layer, the antiphase domain defects can be suppressed. In this way, while taking advantage of the better lattice match between the Ge substrate and the AlGaAs material of the N-type DBR reflective layer to reduce stress and warping and improve device uniformity, the generation of reverse domain defects can be reduced or avoided.

[0089] In this specification, each part is described in a combined manner of parallelism and progression. The key points of each part are the differences from other parts. For the same or similar parts among the parts, reference can be made to each other.

[0090] Regarding the above description of the disclosed embodiments, the features described in each embodiment of this specification can be replaced or combined with each other, enabling those skilled in the art to implement or use the present application. Various modifications to these embodiments will be obvious to those skilled in the art. The general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the broadest scope consistent with the principles and novel features disclosed herein.

Claims

1. A vertical cavity surface emitting laser, characterized in that: include: An N-type Ge substrate, wherein the crystal orientation of the N-type Ge substrate is 100 plane and the deviation from 111 plane is greater than or equal to 2°; A defect suppression layer located on one side of the N-type Ge substrate, wherein the defect suppression layer is an AlGaInP layer, an AlInP layer or a GaInP layer; The defect suppression layer is located on the side away from the N-type Ge substrate, and the N-type DBR reflection layer, the first restriction layer, the active layer, the second restriction layer, the oxidation restriction layer and the P-type DBR reflection layer are stacked in a direction away from the N-type Ge substrate; the N-type DBR reflection layer includes a first refractive index layer and a second refractive index layer stacked alternately, and the first refractive index layer is Al x GaAs layer, the second refractive index layer is Al y GaAs layer, x <y。 2. The vertical cavity surface emitting laser according to claim 1, characterized in that: The In composition of the defect suppression layer is in the range of 0.5% to 0.7%, both inclusive.

3. The vertical cavity surface emitting laser according to claim 1, characterized in that: The defect suppression layer is an AlGaInP layer or an AlInP layer, and the Al component of the defect suppression layer is greater than 20%.

4. The vertical cavity surface emitting laser according to claim 1, characterized in that: The defect suppression layer has a thickness ranging from 5 nm to 200 nm, both inclusive.

5. The vertical cavity surface emitting laser according to any one of claims 1 to 4, characterized in that: The defect suppression layer is doped with a surfactant, and the material of the surfactant is a Sb material or a Te material.

6. A method for preparing a vertical cavity surface emitting laser, characterized in that: include: Providing an N-type Ge substrate, wherein the crystal orientation of the N-type Ge substrate is 100 plane and the deviation from 111 plane is greater than or equal to 2°; forming a defect suppression layer on one side of the N-type Ge substrate, wherein the defect suppression layer is an AlGaInP layer, an AlInP layer or a GaInP layer, and the growth temperature range of the defect suppression layer is 650° C.-700° C., including end points; On the side of the defect suppression layer away from the N-type Ge substrate, a stacked N-type DBR reflection layer, a first restriction layer, an active layer, a second restriction layer, an oxidized restriction layer and a P-type DBR reflection layer are formed in a direction away from the N-type Ge substrate; the N-type DBR reflection layer includes a first refractive index layer and a second refractive index layer alternately stacked, and the first refractive index layer is Al x GaAs layer, the second refractive index layer is Al y GaAs layer, x <y。 7. The method for preparing a vertical cavity surface emitting laser according to claim 6, characterized in that: The In composition of the defect suppression layer is in the range of 0.5% to 0.7%, both inclusive.

8. The method for preparing a vertical cavity surface emitting laser according to claim 6, characterized in that: The defect suppression layer is an AlGaInP layer or an AlInP layer, and the Al component of the defect suppression layer is greater than 20%.

9. The method for preparing a vertical cavity surface emitting laser according to claim 6, characterized in that: The defect suppression layer has a thickness ranging from 5 nm to 200 nm, both inclusive.

10. The method for preparing a vertical cavity surface emitting laser according to any one of claims 6 to 9, characterized in that: When forming the defect suppression layer, a surfactant is doped into the defect suppression layer, and the material of the surfactant is a Sb material or a Te material.

Citation Information

Cited By

  • Laser epitaxial wafer

    CN121216226A