Solar cell and preparation method thereof, photovoltaic module and photovoltaic system
By using C1-5 alkyl passivator in perovskite solar cells to form the passivation layer, the stability problem of perovskite film is solved, the photoelectric performance and stability are improved, and the defects of water molecules and Pb2+ are achieved. Effective protection.
Patent Information
- Application Number
- CN202411044434.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
Perovskite solar cells have poor stability due to their high defect density at the interface, low ion transfer barriers, and the inherent hydrophilicity of the materials, and are susceptible to degradation induced by moisture and oxygen, which affects their commercial application.
The passivation layer is formed on the sides of the perovskite layer, and a passivation agent selected from C1 to 5 alkyl groups is used to combine with a passivation agent with a lower surface reactive activity of the three-dimensional perovskite film to protect the perovskite film from water molecules Attack and passivate undercoordinated Pb2+ defects to improve the photoelectric performance and stability of solar cells.
Effectively protecting perovskite films, improving the photoelectric performance, repeatability and stability of solar cells, reducing energy loss and degradation, and improving the overall performance of the device.
Smart Images

Figure CN118973279A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to solar cells and preparation methods thereof, photovoltaic modules and photovoltaic systems. Background Art
[0002] Perovskite solar cells (PSCs) are ideal candidates for next-generation photovoltaic devices due to their excellent efficiency, feasible processability, and good compatibility with large-scale deposition techniques. However, PSCs face long-term instability issues, which remains a key obstacle to overcome for their commercialization.
[0003] The interface of perovskite film has high defect density and low ion transfer barrier, and the inherent hydrophilicity of perovskite film material makes it susceptible to moisture and oxygen-induced degradation, which will lead to poor operational stability of PSC and further cause energy loss and degradation in PSC. Summary of the invention
[0004] In view of the technical problems existing in the background technology, the present application provides a solar cell, aiming to improve the performance of the solar cell.
[0005] In order to achieve the above-mentioned object, the first aspect of the present application provides a solar cell, wherein the solar cell comprises:
[0006] Perovskite layer;
[0007] A passivation layer, the passivation layer is located on one side of the perovskite layer, the passivation layer includes a passivator, and the passivator includes Wherein, R is selected from C 1~5 alkyl;
[0008] A carrier transport layer is located on a side of the passivation layer away from the perovskite layer.
[0009] The present invention at least has the following beneficial effects: the passivator in the solar cell of the present invention has low surface reaction activity with the three-dimensional perovskite film, is not easy to penetrate the perovskite film and diffuse into the perovskite bulk phase, protects the perovskite film from attack by water molecules and passivates the under-coordinated Pb 2+ defects and improve the photoelectric performance, repeatability and stability of solar cells.
[0010] In some embodiments of the present application, the passivating agent includes
[0011] And / or, R is selected from methyl, ethyl, propyl or isopropyl.
[0012] In some embodiments of the present application, the passivating agent includes
[0013] In some embodiments of the present application, the thickness of the passivation layer is 1 nm to 5 nm.
[0014] In some embodiments of the present application, the carrier transport layer includes an electron transport layer.
[0015] In some embodiments of the present application, the perovskite layer includes a perovskite material having a structural formula of ABX3, wherein the A-position cation includes a formamidinium ion; the B-position cation includes a lead ion; and the X-position anion includes one or more of a chloride ion, a bromide ion, and an iodide ion.
[0016] In some embodiments of the present application, the A-site cation further comprises at least one of a cesium ion and a methylamine ion;
[0017] The molar percentage of the formamidinium ions in the total cations at the A site is 75% to 85%, the molar percentage of the cesium ions in the total cations at the A site is 10% to 20%, and the molar percentage of the methylamine ions in the total cations at the A site is 0% to 10%;
[0018] And / or, the X-site anions include bromide ions and iodide ions, the bromide ions account for 10% to 30% of the total molar percentage of the X-site anions, and the iodide ions account for 70% to 90% of the total molar percentage of the X-site anions.
[0019] In some embodiments of the present application, a buffer layer is provided on a side of the carrier transport layer away from the perovskite layer.
[0020] In some embodiments of the present application, the solar cell includes: a bottom cell, wherein the bottom cell is located on a side of the perovskite layer away from the passivation layer.
[0021] In a second aspect of the present application, the present application proposes a method for preparing the solar cell described in the first aspect, the method comprising: forming the passivation layer between the carrier transport layer and the perovskite layer.
[0022] In some embodiments of the present application, the method comprises:
[0023] forming a perovskite layer on one side of the substrate;
[0024] forming a passivation layer on a side of the perovskite layer away from the substrate;
[0025] forming a carrier transport layer on a side of the passivation layer away from the perovskite layer;
[0026] Wherein, forming the passivation layer comprises: applying a solution containing the passivating agent to a side of the perovskite layer away from the substrate and annealing;
[0027] The concentration of the passivator in the solution containing the passivator is 2 mg / mL to 15 mg / mL.
[0028] In the third aspect of the present application, the present application proposes a photovoltaic module, which includes at least one battery string, and the battery string includes at least two solar cells described in the first aspect of the present application, or a solar cell prepared by the method for preparing a solar cell described in the second aspect of the present application.
[0029] In a fourth aspect of the present application, the present application provides a photovoltaic system, wherein the photovoltaic system comprises the photovoltaic component described in the third aspect of the present application.
[0030] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0032] Figure 1 This is a schematic diagram of the structure of a solar cell according to one embodiment of the present application;
[0033] Figure 2 The figure is a schematic diagram of a process for preparing a solar cell according to an embodiment of the present application.
[0034] Description of reference numerals:
[0035] 10: solar cell; 100: perovskite layer; 200: passivation layer; 300: carrier transport layer; 310: electron transport layer; 320: hole transport layer; 400: buffer layer; 500: transparent conductive layer; 600: electrode layer; 700: substrate. DETAILED DESCRIPTION
[0036] The following is a detailed description of the embodiments of the technical solution of the present application. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0037] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0038] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 listed, and if the maximum range values 3,4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers, and the scope limited in this way can be including end values a and b. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0039] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0040] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0041] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0042] The interface of perovskite film has high defect density and low ion transfer barrier, and the inherent hydrophilicity of perovskite film material makes it susceptible to moisture and oxygen-induced degradation, which will lead to poor operational stability of PSC and further cause energy loss and degradation in PSC.
[0043] In the prior art, the surface of the perovskite film is passivated by forming a 2D and 3D hybrid structure at the interface, in which a thin layer of Ruddlesden-Popper 2D perovskite terminates the 3D perovskite surface. These 2D / 3D structures are constructed by exposing the surface of the perovskite film to a solution containing ammonium ligands, during which the 3D lattice is broken into 2D layers. However, under high temperature conditions, the reactivity of ammonium ligands with 3D perovskites may cause the ammonium ligands to further penetrate into the bulk perovskite film and may lead to deterioration of device performance. At the same time, most stable passivators have limited passivation capabilities on the perovskite surface.
[0044] To this end, the first aspect of the present application proposes a solar cell, see Figure 1 , the solar cell 10 comprises:
[0045] Perovskite layer 100;
[0046] The passivation layer 200 is located on one side of the perovskite layer 100, and the passivation layer 200 includes a passivator, and the passivator includes Where R is selected from C 1~5 alkyl;
[0047] The carrier transport layer 300 is located on a side of the passivation layer 200 away from the perovskite layer 100 .
[0048] The aniline in the passivator of the solar cell of the present invention has a low reactivity with the three-dimensional perovskite and is not easy to penetrate the perovskite film and diffuse into the perovskite bulk phase. At the same time, the strong hydrophobic fluoromethyl tail of the passivator can protect the perovskite film from the attack of water molecules. In addition, the morpholine structure of the passivator can cooperate with fluorine atoms to passivate the under-coordinated Pb 2+ defects, and jointly improve the photovoltaic performance, repeatability and stability of solar cells.
[0049] In some embodiments of the present application, the passivating agent includes The above passivators have low reactivity with three-dimensional perovskites and are not easy to penetrate the perovskite film and diffuse into the perovskite bulk phase, which can better protect the perovskite film from the attack of water molecules and passivate the under-coordinated Pb 2+Among them, placing the amino group and the morpholine group at the meta position or para position of -R-CH3 can further avoid the passivation effect being affected by the strong electronegativity of the fluorine atom.
[0050] In some embodiments of the present application, R is selected from methyl, ethyl, propyl or isopropyl.
[0051] In some embodiments of the present application, the passivating agent includes (3-morpholine-5-(trifluoromethyl)aniline, CAS No. 641571-02-0), (4-morpholine-3-(trifluoromethyl)aniline, CAS No. 105316-06-1) or (3-amino-4-(4-morpholinyl) trifluorotoluene, CAS No. 784-57-6). The above passivating agent has low reactivity with three-dimensional perovskite and is not easy to penetrate the perovskite film and diffuse into the perovskite bulk phase, which can better protect the perovskite film from the attack of water molecules and passivate the under-coordinated Pb 2+ defects to further improve the photovoltaic performance, repeatability and stability of solar cells.
[0052] In some embodiments of the present application, the thickness of the passivation layer 200 is 1 nm to 5 nm, for example, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, etc. The thickness of the passivation layer meets the given conditions, which can promote carrier transport, avoid interface non-radiative recombination, increase the fill factor, and improve the stability and performance of the solar cell.
[0053] In some embodiments of the present application, see Figure 1 , the carrier transport layer 300 may include an electron transport layer 310 or a charge transport layer 320. Exemplarily, the carrier transport layer 300 includes an electron transport layer 310. By providing a passivation layer between the perovskite layer and the electron transport layer, the passivation agent in the passivation layer has a low reactivity with the three-dimensional perovskite, and is not easy to penetrate the perovskite film and diffuse into the perovskite bulk phase, which can better protect the perovskite film from the attack of water molecules and passivate the under-coordinated Pb 2+ Defects can be eliminated to further improve the photoelectric performance, repeatability and stability of solar cells. The photoelectric performance, repeatability and stability of solar cells can be improved as a whole.
[0054] In some embodiments of the present application, the perovskite layer 100 includes a perovskite material having a structural formula of ABX3, wherein the A-site cation includes a formamidinium ion; the B-site cation includes a lead ion; and the X-site anion includes one or more of a chloride ion, a bromide ion, and an iodide ion. The fluorine atom and the morpholinyl group in the passivator can synergistically passivate the undercoordinated Pb2+ defects, thus improving the photoelectric performance, repeatability and stability of solar cells as a whole.
[0055] In some embodiments of the present application, the A-site cations further include at least one of cesium ions and methylamine ions; the formamidinium ions account for 75% to 85% of the total molar percentage of the A-site cations, the cesium ions account for 10% to 20% of the total molar percentage of the A-site cations, and the methylamine ions account for 0% to 10% of the total molar percentage of the A-site cations. In some embodiments, the formamidinium ions account for 78%, 80%, 82%, etc. of the total molar percentage of the A-site cations, the cesium ions account for 12%, 15%, 18% of the total molar percentage of the A-site cations, and the methylamine ions account for 2%, 4%, 6%, 8% of the total molar percentage of the A-site cations. The formamidinium ions, cesium ions, and methylamine ions meet the given conditions, can promote the uniform growth of perovskite crystals, reduce crystal defects, and have high film quality.
[0056] In some embodiments of the present application, the X-site anions include bromide ions and iodide ions, the bromide ions account for 10% to 30% of the total molar percentage of the X-site anions, and the iodide ions account for 70% to 90% of the total molar percentage of the X-site anions. In some embodiments, the bromide ions account for 15%, 20%, 25%, 28%, etc. of the total molar percentage of the C-site cations, and the iodide ions account for 75%, 80%, 85%, etc. of the total molar percentage of the X-site anions. Bromide ions and iodide ions meet the given conditions, can promote the uniform growth of perovskite crystals, reduce crystal defects, and have high film quality.
[0057] In some embodiments of the present application, the electron transport layer 310 includes: one or more of fullerene and its derivatives, cyanide-containing polyphenylene vinylene, boron-containing polymers, 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline, 4,7-diphenyl-1,10-phenanthroline, hydroxyquinoline aluminum, oxadiazole compounds, benzimidazole compounds, naphthalenetetracarboxylic acid compounds, perylene derivatives, phosphine oxide compounds, phosphine sulfide compounds, fluorinated phthalocyanine, titanium oxide, zinc oxide, indium oxide, tin oxide, gallium oxide, tin sulfide, indium sulfide, lithium fluoride, sodium fluoride, magnesium fluoride, calcium fluoride and zinc sulfide.
[0058] In some embodiments of the present application, the solar cell 10 further includes: a hole transport layer 320 , and the hole transport layer 320 is located on a side of the perovskite layer 100 away from the passivation layer 200 .
[0059] In some embodiments of the present application, the hole transport layer 320 includes: [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid, benzoic acid, 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid, [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], 4,4'-cyclohexylbis[N,N-bis(4-methylphenyl)aniline, 2,2", 7,7"-Tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, [bis(4-phenyl)(2,4,6-trimethylphenyl)amine], poly(3-hexylthiophene-2,5-diyl), poly(3,4-ethylenedioxythiophene): poly(4-styrenesulfonic acid), 2,2',7,7'-tetrakis(N,N-di-p-tolyl)amino-9,9'-spirobifluorene, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanodimethyl-p-benzoquinone, hexafluoro-2,3,5,6-tetracyano-4-benzothiazoline, 4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline], NiO x , CuSCN, CuAlO2, V2O5, CdS and CdSe.
[0060] Therefore, the use of the above hole transport layer materials and electron transport layer materials can improve the photoelectric performance, repeatability and stability of the stacked solar cells.
[0061] In some embodiments of the present application, see Figure 1 , a buffer layer 400 is provided on the side of the carrier transport layer 300 away from the perovskite layer 100. By providing the buffer layer 400 to improve charge transfer, adjust energy level arrangement, and provide physical and chemical stability, it is also possible to reduce interface defects, improve light absorption efficiency and flexibility, and promote the formation of heterostructures, thereby improving the photoelectric conversion efficiency and stability of solar cells. Exemplarily, the buffer layer includes 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP).
[0062] In some embodiments of the present application, the solar cell 10 further includes: a transparent conductive layer 500, an electrode layer 600 and a substrate 700, the transparent conductive layer 500 is located on a side of the hole transport layer 320 away from the perovskite layer 100, the electrode layer 600 is located on a side of the buffer layer 400 away from the perovskite layer 100, and the substrate 700 is located on a side of the transparent conductive layer 500 away from the perovskite layer 100.
[0063] In some embodiments of the present application, the conductive material of the transparent conductive layer 500 includes one or more of gallium zinc oxide, aluminum zinc oxide, indium zinc oxide, fluorine-doped tin oxide, indium tin oxide, barium stannate, titanium-doped tin oxide, and zinc-doped tin oxide.
[0064] In some embodiments of the present application, the material of the electrode layer 600 includes one or more of gold, silver, copper and aluminum.
[0065] In some embodiments of the present application, the substrate 700 includes glass.
[0066] In some embodiments of the present application, the solar cell 10 includes: a bottom cell, the bottom cell is located on a side of the perovskite layer away from the passivation layer. In some embodiments, the bottom cell includes any one of a crystalline silicon bottom cell, a polycrystalline silicon bottom cell, a cast monocrystalline silicon bottom cell, a copper indium gallium selenide bottom cell, a perovskite bottom cell, a gallium arsenide bottom cell, and an organic photovoltaic bottom cell.
[0067] In a fourth aspect of the present application, the present application proposes a method for preparing the solar cell described in the third aspect of the present application, the method comprising: forming the passivation layer between the carrier transport layer and the perovskite layer.
[0068] In some embodiments of the present application, see Figure 2 The method includes: forming a perovskite layer in step S100, forming a passivation layer in step S200, and forming a carrier transport layer in step S300. Each step will be described in detail below.
[0069] S100 forms a perovskite layer
[0070] In this step, a perovskite layer is formed on one side of the substrate.
[0071] In some embodiments of the present application, the method of forming the perovskite layer includes: spin coating a perovskite precursor solution onto one side of a substrate, and annealing to form the perovskite layer;
[0072] The perovskite precursor solution contains A-site cations, B-site cations, X-site anions and a solvent, and the solvent is selected from dimethyl sulfoxide and N,N-dimethylformamide in a volume ratio of (0-5):10, or dimethyl sulfoxide, N-methylpyrrolidone and N,N-dimethylformamide in a volume ratio of 1:(0-1):(8-9). In some embodiments, the volume ratio of dimethyl sulfoxide and N,N-dimethylformamide is (1-4):10 or (2-3):10, and the volume ratio of dimethyl sulfoxide, N-methylpyrrolidone and N,N-dimethylformamide is 1:(0.3-0.6):(8.3-8.6).
[0073] S200 forms a passivation layer
[0074] In this step, a passivation layer is formed on a side of the perovskite layer away from the substrate.
[0075] In some embodiments of the present application, the method of forming the passivation layer includes: applying a solution containing a passivating agent to a side of the perovskite layer away from the substrate and annealing;
[0076] Wherein, the concentration of the passivator in the solution containing the passivator is 2 mg / mL to 15 mg / mL. In some embodiments, the concentration of the passivator in the solution containing the passivator is 2 mg / mL, 4 mg / mL, 5 mg / mL, 8 mg / mL, 10 mg / mL, 12 mg / mL, 14 mg / mL, 15 mg / mL, etc. The concentration of the passivator meets the given conditions, which can improve the open circuit voltage, fill factor and photoelectric conversion efficiency of the solar cell, facilitate charge extraction, and improve the performance of the solar cell.
[0077] S300 forms a carrier transport layer
[0078] In this step, a carrier transport layer is formed on a side of the passivation layer away from the perovskite layer.
[0079] In the third aspect of the present application, the present application proposes a photovoltaic module, comprising at least one battery string, wherein the battery string comprises at least two solar cells described in the first aspect of the present application, or a solar cell prepared by the method for preparing a solar cell described in the second aspect of the present application. Therefore, the photovoltaic module has all the features and advantages of the aforementioned solar cell, which will not be described in detail here.
[0080] In some embodiments, the solar cells may be connected together by serial welding, so that the electric energy generated by the individual solar cells can be collected for subsequent transmission.
[0081] In some embodiments, the solar cells may be arranged at intervals or stacked together in a shingled form.
[0082] For example, the photovoltaic module further includes an encapsulation layer and a cover plate, wherein the encapsulation layer is used to cover the surface of the battery string, and the cover plate is used to cover the surface of the encapsulation layer away from the battery string.
[0083] In the fourth aspect of the present application, the present application proposes a photovoltaic system, including the photovoltaic assembly described in the first aspect of the present application. Therefore, the photovoltaic system has all the features and advantages of the aforementioned photovoltaic assembly, which will not be described in detail here.
[0084] Photovoltaic systems can be used in photovoltaic power stations, such as ground power stations, rooftop power stations, water power stations, etc., and can also be used in equipment or devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars, solar buildings, etc. Of course, it is understandable that the application scenarios of photovoltaic systems are not limited to this, that is to say, photovoltaic systems can be used in all fields that require solar energy to generate electricity. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.
[0085] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.
[0086] Example 1
[0087] First, select 20 ohm ITO glass and clean it with deionized water, ethanol and detergent before use; then sputter NiOx with a thickness of 20nm; UV is required for 20 minutes before sputtering to remove organic impurities, and then solution-coated [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz): [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid = 3:1 as a hole transport layer with a thickness of 5nm; then FAI powder, MAI powder, CsI powder, PbBr2 and PbI2 powder are mixed in a certain proportion and dissolved in a mixed solution of DMF / DMSO (volume ratio DMF:DMSO = 4:1), with a configuration ratio of FA 0.8 Cs 0.15 MA 0.05 Pb(Br 0.25 I 0.75 )3 The perovskite precursor solution, with a band gap of about 1.68 eV, was spin-coated by a one-step anti-solvent method, with anisole as the anti-solvent, and annealed at 100°C for 20 min to obtain a perovskite film with a thickness of 500 nm; then, a passivation agent was dynamically spin-coated on the perovskite film by a solution method solution, concentration of 10 mg / ml, annealed at 100 °C for 5 min, thickness of 3 nm; finally, C was sputtered on the perovskite film 60As an electron transport layer with a thickness of 30nm, BCP is then sputtered as a buffer layer with a thickness of 6nm, and finally Ag is sputtered with a thickness of 150nm to prepare a device.
[0088] Example 2
[0089] The difference from Example 1 is that the passivating agent is
[0090] Example 3
[0091] The difference from Example 1 is that the passivating agent is
[0092] Comparative Example 1
[0093] Different from Example 1, C is directly sputtered on the perovskite film. 60 As an electron transport layer, no passivating agent is applied.
[0094] Comparative Example 2
[0095] The difference from Example 1 is that the passivating agent is
[0096] Comparative Example 3
[0097] The difference from Example 1 is that the passivating agent is
[0098] Comparative Example 4
[0099] The difference from Example 1 is that the passivating agent is
[0100] Test Case
[0101] The performance tests were performed on the solar cell devices prepared in the above Examples 1 to 3 and Comparative Examples 1 to 4 respectively.
[0102] The specific test method is: place the prepared battery device under a light source with an intensity P of 100mW / cm 2The AM1.5G standard simulates sunlight. By changing the bias voltage of the load on the battery device, the current value of the battery device is obtained, thereby drawing the current density (J)-voltage (V) curve of the battery device, and thus obtaining the open circuit voltage Voc, short circuit current density Jsc, fill factor FF, and photoelectric conversion efficiency of the battery device, that is, battery efficiency PCE: V and J of the battery device change with the change of external load. When the external load is short-circuited, V=0, and J at this time is called short-circuit current density Jsc; when the external load is disconnected, J=0, and V at this time is called open circuit voltage Voc; the output power of the battery device has a maximum value, which is called the maximum power point Pmax, Pmax divided by the effective light-receiving area of the battery device, that is, the battery efficiency PCE; the fill factor FF of the battery device is PCE×P / (Jsc×Voc).
[0103] As shown in Table 1, the performance of the solar cells of Examples 1 to 3 is significantly better than that of Comparative Examples 1 to 4, indicating that the use of the passivating agent of the present application can effectively improve the photoelectric performance, repeatability and stability of the solar cells.
[0104] Table 1 Performance parameters of different solar cells
[0105]
[0106]
[0107] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A solar cell, characterized in that: include: Perovskite layer; A passivation layer, the passivation layer is located on one side of the perovskite layer, the passivation layer includes a passivator, and the passivator includes Where R is selected from C 1~5 alkyl; A carrier transport layer is located on a side of the passivation layer away from the perovskite layer.
2. The solar cell according to claim 1, characterized in that The passivating agent includes And / or, R is selected from methyl, ethyl, propyl or isopropyl.
3. The solar cell according to claim 1, characterized in that The passivating agent includes 4. The solar cell according to claim 1, characterized in that The thickness of the passivation layer is 1 nm to 5 nm.
5. The solar cell according to claim 1, characterized in that: The carrier transport layer includes an electron transport layer.
6. The solar cell according to claim 1, characterized in that The perovskite layer includes a perovskite material having a structural formula of ABX3, wherein the A-site cation includes a formamidinium ion; the B-site cation includes a lead ion; and the X-site anion includes one or more of a chloride ion, a bromide ion and an iodide ion.
7. The solar cell according to claim 6, characterized in that: The A-site cation further comprises at least one of a cesium ion and a methylamine ion; The molar percentage of the formamidinium ions in the total cations at the A site is 75% to 85%, the molar percentage of the cesium ions in the total cations at the A site is 10% to 20%, and the molar percentage of the methylamine ions in the total cations at the A site is 0% to 10%; And / or, the X-site anions include bromide ions and iodide ions, the bromide ions account for 10% to 30% of the total molar percentage of the X-site anions, and the iodide ions account for 70% to 90% of the total molar percentage of the X-site anions.
8. The solar cell according to claim 1, characterized in that A buffer layer is provided on a side of the carrier transport layer away from the perovskite layer.
9. The solar cell according to claim 1, characterized in that: include: A bottom cell is located on a side of the perovskite layer away from the passivation layer.
10. A method for preparing the solar cell according to any one of claims 1 to 9, characterized in that: include: The passivation layer is formed between the carrier transport layer and the perovskite layer.
11. The method according to claim 10, characterized in that include: forming a perovskite layer on one side of the substrate; forming a passivation layer on a side of the perovskite layer away from the substrate; forming a carrier transport layer on a side of the passivation layer away from the perovskite layer; Wherein, forming the passivation layer comprises: applying a solution containing the passivating agent to a side of the perovskite layer away from the substrate and annealing; The concentration of the passivator in the solution containing the passivator is 2 mg / mL to 15 mg / mL.
12. A photovoltaic module, characterized in that: The invention comprises at least one battery string, wherein the battery string comprises at least two solar cells according to any one of claims 1 to 9, or a solar cell prepared by the method according to claim 10 or 11.
13. A photovoltaic system, characterized in that: include: The photovoltaic module according to claim 12.