Rolling bonded body and method for manufacturing same

Through the surface activation bonding method and control interface conditions, the problem of the existing calendered joint between high peel strength and bending resistance is solved, and the efficient bonding and bending performance of the aluminum layer and the copper layer is achieved, thereby avoiding the intermetallic compound The production improves the overall performance of the calendered joint.

CN118973754APending Publication Date: 2024-11-15TOYO KOHAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031498.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing calendered joint composed of an aluminum layer and a copper layer is difficult to have high resistance to bonding and bending processing while having high peel strength. The heat treatment will lead to the formation of intermetallic compounds, reduce the peel strength and cause cracking and peeling problems.

Method used

The calendered joint is made by surface activation bonding method. By sputtering etching of aluminum plates and copper plates and bonding without heat treatment or under 250°C, the aluminum layer and copper layer are controlled. The hardness and surface thickness of the layer achieve high peel strength and high resistance.

Benefits of technology

It achieves high peel strength and high resistance at the intermetallic compound-free interface, and is suitable for bonding wires, bonding tapes and bending processing, reducing damage to semiconductor chips and improving the overall performance of the calendered joint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973754A_ABST
    Figure CN118973754A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a rolled bonded body having both high peel strength and high resistance to bonding and bending. The present invention pertains to: a rolled bonded body comprising an aluminum layer and a copper layer, in which there is no intermetallic compound containing aluminum and copper at the interface between the aluminum layer and the copper layer, and in which the peel strength exceeds 10 N / cm;
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rolled bonded body and a method for producing the same. Background Art

[0002] Power modules are used in various products such as industrial machinery, home appliances, and information terminals. Various metal materials are used for the bonding wires and bonding ribbons used in power modules. As such metal materials, rolled composite bodies (also called metal laminated materials, cladding materials) formed by stacking two or more metal plates or metal foils are known. Rolled composite bodies are highly functional metal materials with composite properties that cannot be obtained by relying on a single material. For example, rolled composite bodies composed of aluminum layers and copper layers are being studied (Patent Documents 1 to 5).

[0003] The rolled bonded body used for the bonding wire and bonding tape used in the power module needs to have various characteristics depending on the purpose of the power module. For example, it needs to have high peel strength (also called bonding strength) and high resistance to bonding and bending. In the current rolled bonded body composed of an aluminum layer and a copper layer, in order to fully improve the peel strength of the rolled bonded body, a heat treatment above a certain temperature is generally required. However, this heat treatment will cause the interface of the aluminum layer and the copper layer to generate intermetallic compounds containing these metals. If there are intermetallic compounds at the interface of the rolled bonded body, the peel strength will decrease, and it may cause adverse effects such as cracking and peeling during bonding and bending.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-227241

[0007] Patent Document 2: International Publication No. 2011 / 155379

[0008] Patent Document 3: Japanese Patent Application Publication No. 2015-226928

[0009] Patent Document 4: International Publication No. 2016 / 63744

[0010] Patent Document 5: Japanese Patent Application Publication No. 2003-80621 Summary of the invention

[0011] Problems to be solved by the invention

[0012] As described above, it is difficult for a conventional rolled bonded body composed of an aluminum layer and a copper layer to have high peel strength and high resistance to bonding and bending. Therefore, an object of the present invention is to provide a rolled bonded body having both high peel strength and high resistance to bonding and bending.

[0013] Technical solutions for solving technical problems

[0014] The present inventors conducted intensive studies to solve the above-mentioned problems and found that by manufacturing a rolled bonded body using a surface activated bonding method in which heat treatment is controlled, it is possible to achieve both high peel strength and high resistance to bonding and bending in the rolled bonded body, thereby completing the present invention.

[0015] That is, the gist of the present invention is as follows.

[0016] (1) A rolled bonded body comprising an aluminum layer and a copper layer, wherein an intermetallic compound containing aluminum and copper does not exist at an interface between the aluminum layer and the copper layer, and the peel strength exceeds 10 N / cm.

[0017] (2) The rolled bonded body according to the above (1), wherein the aluminum layer has a hardness HV of 40 or less.

[0018] (3) The rolled joint body according to (1) or (2) above, wherein the surface roughness Rz of the aluminum layer is 0.5 μm or less.

[0019] (4) The rolled joint body according to any one of (1) to (3) above, wherein the aluminum is 1000 series pure aluminum specified in JIS.

[0020] (5) The rolled joint body according to any one of (1) to (4) above, wherein the copper layer has a hardness HV of 130 or less.

[0021] (6) The rolled joint body according to any one of (1) to (5) above, wherein the copper is 1000 series pure copper specified in JIS.

[0022] (7) The rolled joint body according to any one of (1) to (6) above, wherein a ratio of the hardness of the copper layer to the hardness of the aluminum layer (hardness of the copper layer / hardness of the aluminum layer) is 1.0 to 5.0.

[0023] (8) The rolled bonded body according to any one of (1) to (7) above, wherein the rolled bonded body is in a linear or belt-like shape.

[0024] (9) A method for producing a rolled bonded body, wherein the rolled bonded body is the rolled bonded body according to any one of (1) to (8) above, the method comprising the following steps:

[0025] Sputter etching of aluminum plates;

[0026] sputter etching the copper plate; and,

[0027] The surfaces of the aluminum plate and the copper plate after sputtering etching are press-bonded to each other so that the rolling reduction rate of the rolled joint body reaches 3% or more,

[0028] After the step of joining, no heat treatment is performed, or a heat treatment below 250° C. is performed.

[0029] (10) A bonding wire or a bonding tape, comprising the rolled bonded body according to any one of (1) to (8) above.

[0030] This specification incorporates the disclosure of Japanese Patent Application No. 2022-058644 which is the basis of priority for this application.

[0031] Effects of the Invention

[0032] According to the present invention, a rolled bonded body having both high peel strength and high resistance to bonding and bending can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1-1 1A to 1D show the results of confirming whether there are intermetallic compounds in the examples; FIG. 1A is a cross-sectional SEM image (2000 times) of the rolled joint of Example 1; and FIG. 1B is a cross-sectional SEM image (2000 times) of the rolled joint of Example 2.

[0034] Figure 1-2 1A to 1D show the results of confirming whether there are intermetallic compounds in the examples; FIG. 1C is a cross-sectional SEM image (2000 times) of the rolled joint of Comparative Example 1; and FIG. 1D is a cross-sectional SEM image (2000 times) of the rolled joint of Comparative Example 4.

[0035] Figure 2 middle, Figure 2 A to C show the results of confirming whether cracks caused by bending and rebending exist in the examples; Figure 2 A is a cross-sectional SEM image (2000 times) of the rolled joint body of Example 1; Figure 2 B is a cross-sectional SEM image (2000 times) of the rolled joint body of Example 2; Figure 2 C is a cross-sectional SEM image of the rolled bonded body of Comparative Example 1 (magnification 2000). DETAILED DESCRIPTION

[0036] The present invention is described in detail below: The present invention relates to a rolled bonded body having a double-layer structure of an aluminum layer and a copper layer, that is, to a rolled bonded body composed of an aluminum layer and a copper layer in which an aluminum layer and a copper layer are directly laminated.

[0037] The aluminum used for the aluminum layer may be pure aluminum or an aluminum alloy, but pure aluminum is preferred from the viewpoint of flexibility and conductivity when used for a bonding wire or a bonding ribbon.

[0038] The purity of pure aluminum is usually 99.0% by mass or more, preferably 99.5% by mass or more. The total content of added metal elements other than aluminum in pure aluminum is usually 1.0% by mass or less, preferably 0.7% by mass or less, more preferably 0.5% by mass or less, and particularly preferably 0.3% by mass or less. As pure aluminum, for example, 1000 series pure aluminum specified in JIS (JIS-H4000) can be used, preferably A1100, A1N30, A1050, A1085, A1N99.

[0039] As the aluminum alloy, an aluminum alloy in which the total content of metal elements other than aluminum exceeds 1 mass %, for example, an aluminum alloy containing at least one added metal element selected from Mg, Mn, Si and Cu in the form of a total content of the added metal elements exceeding 1 mass % can be used.

[0040] As aluminum alloys, for example, Al-Cu alloys (2000 series), Al-Mn alloys (3000 series), Al-Si alloys (4000 series), Al-Mg alloys (5000 series), Al-Mg-Si alloys (6000 series) and Al-Zn-Mg alloys (7000 series) specified in JIS can be used. From the viewpoints of stamping formability, strength and corrosion resistance, aluminum alloys of the 3000 series, 5000 series, 6000 series and 7000 series are preferred, and from the viewpoints of strength and conductivity, aluminum alloys of the 3000 series are more preferred.

[0041] The thickness of the aluminum layer can generally be used if it is 0.01 mm or more. From the perspective of processability and handling of the rolled joint body, the lower limit is preferably 0.03 mm or more. If strength is also required, it is more preferably 0.05 mm or more. From the perspective of lightweight and cost, the thickness of the aluminum layer is preferably 1.0 mm or less, more preferably 0.5 mm or less, and particularly preferably 0.3 mm or less. The thickness of the aluminum layer is preferably 0.01 mm to 1.0 mm, more preferably 0.01 mm to 0.5 mm, and particularly preferably 0.03 mm to 0.3 mm. The thickness of the aluminum layer is an optical microscope photograph of a cross-section of the rolled joint body, and the average value of the measured values ​​obtained by measuring the thickness of the aluminum layer at any 10 locations in the optical microscope photograph.

[0042] The hardness HV of the aluminum layer is not particularly limited, and is generally 80 or less. From the perspective of bendability, it is preferably 60 or less, more preferably 40 or less, and particularly preferably 30 or less. In particular, by setting the hardness HV of the aluminum layer to a soft material of 30 or less, when the rolled bonded body is used, for example, as a bonding wire and a bonding tape for a power module, the load during ultrasonic bonding with the semiconductor chip can be reduced, thereby reducing damage to the semiconductor chip. The lower limit of the hardness HV of the aluminum layer is not particularly limited, and is generally 10 or more. From the perspective of strength and handling, it is preferably 15 or more, more preferably 20 or more, and particularly preferably 25 or more. The hardness HV of the aluminum layer is preferably 15 to 60, more preferably 15 to 40, and particularly preferably 15 to 30. The hardness of the aluminum layer can be measured using a micro Vickers hardness tester (load 50 gf) in accordance with JIS Z 2244 (Vickers hardness test-test method).

[0043] The surface roughness Ra of the aluminum layer is not particularly limited, but is preferably 0.5 μm or less, more preferably 0.1 μm or less, and particularly preferably 0.05 μm or less. The surface roughness Ra can be measured using SURFCOM 1400D-3DF (manufactured by Tokyo Seimitsu Co., Ltd.) in accordance with JIS-B0601-1994.

[0044] The surface roughness Rz of the aluminum layer is not particularly limited, but is preferably 0.5 μm or less, more preferably 0.2 μm or less, and particularly preferably 0.1 μm or less. The surface roughness Rz can be measured using SURFCOM 1400D-3DF (manufactured by Tokyo Seimitsu Co., Ltd.) in accordance with JIS-B0601-1994.

[0045] By setting the surface roughness Ra and / or Rz of the aluminum layer to the above range, when the rolled bonded body is used as a bonding wire or a bonding tape for a power module, for example, the adhesion with a semiconductor chip during ultrasonic bonding is excellent, which is preferred.

[0046] The copper used for the copper layer may be pure copper or a copper alloy, but pure copper is preferred from the viewpoint of flexibility and conductivity when used for a bonding wire or a bonding ribbon.

[0047] The purity of pure copper is usually 99.0% by mass or more, preferably 99.5% by mass or more, and more preferably 99.9% by mass or more. The total content of added metal elements other than copper in pure copper is usually 1.0% by mass or less, preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and particularly preferably 0.1% by mass or less. As pure copper, for example, pure copper of the 1000 series specified in JIS can be used, and specifically, oxygen-free copper of JIS-H3510 (C1011) and JIS-H3100 (C1020) specifications specified in JIS can be used, and tough copper of JIS-H3100 (C1100) specifications can be used.

[0048] As the copper alloy, a copper alloy in which the total content of metal elements other than copper exceeds 1 mass% can be used. For example, a copper alloy containing at least one added metal element selected from Sn, Mn, Cr, Zn, Zr, Ni, Si, Mg and Ag as the metal element other than copper in the form of an added metal element with a total content of more than 1 mass% can be used.

[0049] The thickness of the copper layer is generally 0.01 mm or more, and can be used. From the viewpoint of the processability and handling of the rolled joint body, the lower limit is preferably 0.03 mm or more, and if strength is also required, it is more preferably 0.05 mm or more. From the viewpoint of lightweight and cost, the thickness of the copper layer is preferably 1.0 mm or less, more preferably 0.5 mm or less, and particularly preferably 0.3 mm or less. The thickness of the copper layer is preferably 0.01 mm to 1.0 mm, more preferably 0.01 mm to 0.5 mm, and particularly preferably 0.03 mm to 0.3 mm. The thickness of the copper layer can be measured in the same manner as the above-mentioned aluminum layer.

[0050] The hardness HV of the copper layer is not particularly limited, and is generally less than 150. From the perspective of bendability, it is preferably less than 140, and more preferably less than 130. It should be noted that when the rolled joint body is used for wire materials such as conductors that require flexibility, the hardness HV of the copper layer is preferably less than 85, more preferably less than 70, and particularly preferably less than 65. In particular, when the hardness HV of the copper layer is set to a soft material less than 65, as with the above-mentioned aluminum layer, the load during ultrasonic bonding with the semiconductor chip can be reduced, thereby reducing damage to the semiconductor chip. There is no particular restriction on the lower limit of the hardness HV of the copper layer. From the perspective of strength and handling, it is preferably more than 40, more preferably more than 50, and particularly preferably more than 60. The hardness HV of the copper layer is preferably 40 to 140, more preferably 40 to 130, and particularly preferably 40 to 85. The hardness of the copper layer can be measured in the same way as the above-mentioned aluminum layer.

[0051] The closer the ratio of the hardness of the copper layer to the hardness of the aluminum layer (hardness of the copper layer / hardness of the aluminum layer) (hereinafter also referred to as the hardness ratio) is to 1, the more it can withstand more stringent conditions during bending, so it is preferred. The ratio of the hardness of the copper layer to the hardness of the aluminum layer is preferably 1.0 to 5.0, more preferably 1.0 to 4.0, and particularly preferably 1.5 to 3.5. When the hardness ratio is within this range, the hardness of the copper layer and the aluminum layer can be balanced, and even if the conditions during bending are more stringent, the generation and propagation of cracks can be suppressed. The rolled joint body of the present invention has no intermetallic compounds at the interface and has high resistance to bending. Therefore, by controlling the hardness ratio as described above, it can also withstand bending under more stringent conditions. On the other hand, a rolled joint body with intermetallic compounds at the interface will produce cracks in the early stage even when the hardness ratio is close to 1, for example, 1.0 to 2.0, and the cracks will propagate and break, and the resistance to bending under more stringent conditions is low.

[0052] The surface roughness Ra of the copper layer is not particularly limited, but is preferably 0.5 μm or less, more preferably 0.1 μm or less, and particularly preferably 0.05 μm or less. The surface roughness Ra of the copper layer can be measured in the same manner as that of the aluminum layer.

[0053] The surface roughness Rz of the copper layer is not particularly limited, but is preferably 0.5 μm or less, more preferably 0.2 μm or less, and particularly preferably 0.1 μm or less. The surface roughness Rz of the copper layer can be measured in the same manner as the aluminum layer.

[0054] In addition, when the surface roughness Ra and / or Rz of the copper layer is set in the above range, the adhesion with the semiconductor chip during ultrasonic bonding is excellent, similarly to the above-mentioned aluminum layer, which is preferable.

[0055] The rolled bonded body of the present invention is a double-layer material consisting of an aluminum layer and a copper layer. The rolled bonded body of the present invention is a rolled bonded body consisting of an aluminum layer and a copper layer directly stacked. The rolled bonded body of the present invention has no other layer (e.g., a plating layer) between the aluminum layer and the copper layer.

[0056] The rolled joint of the present invention is characterized in that there is no intermetallic compound at the interface of the aluminum layer and the copper layer. In the present invention, the intermetallic compound refers to an intermetallic compound containing aluminum and copper. The absence of intermetallic compounds at the interface of the aluminum layer and the copper layer will improve the resistance to bonding and bending processing. In the present invention, "no intermetallic compound at the interface" means that the interface is magnified to 100 times to 10,000 times (for example, 2,000 times) for observation, and it can be confirmed whether the product at the interface exists, and the state in which the product with a thickness of more than 0.1 μm is not formed on the interface.

[0057] The peel strength of the rolled bonded body of the present invention exceeds 10 N / cm. When the peel strength of the rolled bonded body exceeds 10 N / cm, the aluminum layer and the copper layer will have a sufficiently high adhesion, and the layers will not peel off during bonding and bending, and the rolled bonded body can be used. The peel strength of the rolled bonded body is preferably 15 N / cm or more, more preferably 20 N / cm or more, further preferably 25 N / cm or more, and particularly preferably 30 N / cm or more.

[0058] In the present invention, regarding the peel strength of the rolled joint body, a test piece with a width of 20 mm is prepared from the rolled joint body, and after the aluminum layer and the copper layer are partially peeled off, the thick film layer side or the hard layer side is fixed, and the force required for peeling when the other layer is pulled to the side 180° opposite to the fixed side is measured, and N / cm is used as a unit. It should be noted that in the same test, if the width of the test piece is between 10 mm and 30 mm, the peel strength does not change.

[0059] The thickness of the rolled joint body of the present invention is not particularly limited, and is usually 0.015mm to 1.0mm, and the upper limit is preferably 0.8mm or less, more preferably 0.5mm or less, and particularly preferably 0.3mm or less. The lower limit is preferably 0.02mm or more, and more preferably 0.1mm or more. The thickness of the rolled joint body is preferably 0.02mm to 0.8mm, and particularly preferably 0.05mm to 0.3mm. The thickness of the rolled joint body refers to the total thickness of the aluminum layer and the copper layer. The thickness of the rolled joint body is the average value of the measured values ​​obtained by measuring the thickness of any 10 places on the rolled joint body with a micrometer or the like.

[0060] The shape of the rolled bonded body of the present invention is not particularly limited, and examples thereof include plates, foils, strips, tapes, wires, rings, coils, etc. The rolled bonded body of the present invention has high peel strength and high resistance to bonding and bending, and is preferably in the shape of wires and tapes.

[0061] The present invention also includes a method for manufacturing the above-mentioned rolled bonded body. In the present invention, the rolled bonded body is manufactured by a surface activation bonding method. Specifically, the rolled bonded body of the present invention includes: a step of sputter etching an aluminum plate; a step of sputter etching a copper plate; a step of press-bonding the sputter-etched surfaces of the aluminum plate and the copper plate to each other so that the reduction rate of the rolled bonded body reaches 3% or more. After the bonding step, no heat treatment is performed, or a heat treatment below 250°C, preferably below 220°C, is performed.

[0062] The aluminum plate used in the method for producing a rolled joined body of the present invention is the above-mentioned pure aluminum or aluminum alloy plate material of the aluminum layer of the rolled joined body.

[0063] The thickness of the aluminum plate is generally 0.01 mm or more and can be used. From the viewpoint of the processability and handling of the rolled joint body, the lower limit is preferably 0.03 mm or more. If strength is also required, it is more preferably 0.05 mm or more. From the viewpoint of lightweight and cost, the thickness of the aluminum plate is preferably 1.0 mm or less, more preferably 0.5 mm or less, and particularly preferably 0.3 mm or less. The thickness of the aluminum plate is preferably 0.01 mm to 1.0 mm, more preferably 0.01 mm to 0.5 mm, and particularly preferably 0.03 mm to 0.3 mm. The thickness of the aluminum plate can be measured by a micrometer, etc., and refers to the average value of the thickness measured at 10 randomly selected locations on the surface of the aluminum plate.

[0064] There is no particular restriction on the hardness HV of the aluminum plate, and it is generally 80 or less. From the viewpoint of bendability, it is preferably 60 or less, more preferably 40 or less, and particularly preferably 30 or less. In the surface activation bonding method, soft aluminum plates can be stacked while roughly maintaining hardness. There is no particular restriction on the lower limit of the hardness HV of the aluminum plate, and it is generally 10 or more. From the viewpoint of strength and handling, it is preferably 15 or more, and particularly preferably 20 or more. The hardness HV of the aluminum plate is preferably 15 to 60, and more preferably 15 to 40. In the present invention, the hardness of the aluminum plate can be measured in the same manner as the aluminum layer of the above-mentioned rolled joint body.

[0065] The copper plate used in the method for producing a rolled joined body of the present invention is the above-mentioned pure copper or copper alloy plate material of the copper layer of the rolled joined body.

[0066] The thickness of the copper plate is generally 0.01 mm or more, and can be used. From the viewpoint of the processability and handling of the rolled joint body, the lower limit is preferably 0.03 mm or more, and if strength is also required, it is more preferably 0.05 mm or more. From the viewpoint of lightweight and cost, the thickness of the copper plate is preferably 1.0 mm or less, more preferably 0.5 mm or less, and particularly preferably 0.3 mm or less. The thickness of the copper plate is preferably 0.01 mm to 1.0 mm, more preferably 0.01 mm to 0.5 mm, and particularly preferably 0.03 mm to 0.3 mm. The thickness of the copper plate can be measured in the same manner as the above-mentioned aluminum plate.

[0067] The hardness HV of the copper plate is not particularly limited, and is generally 150 or less. From the viewpoint of bendability, it is preferably 140 or less, and particularly preferably 130 or less. The lower limit of the hardness HV of the copper plate is not particularly limited, and from the viewpoint of strength and handling, it is preferably 40 or more, more preferably 50 or more, and particularly preferably 60 or more. The hardness HV of the copper plate is preferably 40 to 140, and more preferably 40 to 130. In the present invention, the hardness of the copper plate can be measured in the same manner as the aluminum layer of the rolled joint body.

[0068] In the manufacturing method of the present invention, first, the aluminum plate and the copper plate are respectively sputter-etched (sputter-etching treatment step).

[0069] Specifically, the sputtering etching process is to prepare an aluminum plate and a copper plate as a long coil with a width of 100 mm to 600 mm, respectively use the aluminum plate and the copper plate with a joint surface as one of the grounded electrodes, apply an alternating current of 1 MHz to 50 MHz between the other electrodes supported by insulation to generate glow discharge, and set the area of ​​the electrode exposed from the plasma generated by the glow discharge to less than 1 / 3 of the area of ​​the other electrodes. In the sputtering etching process, the grounded electrode has the shape of a cooling roller to prevent the temperature of each conveyed material from rising.

[0070] In the sputtering etching process, the bonding surface of the aluminum plate and the copper plate is sputtered with an inert gas under vacuum to completely remove the adsorbed substances on the surface and remove part or all of the oxide film on the surface. The oxide film does not necessarily have to be completely removed, and sufficient bonding force can be obtained with a portion remaining. By leaving a portion of the oxide film, the sputtering etching process time can be greatly reduced compared to the case of complete removal, thereby improving productivity. Inert gases such as argon, neon, xenon, krypton, and a mixed gas of at least one of these inert gases can be used. Whether it is an aluminum plate or a copper plate, the adsorbed substances on the surface can be completely removed with an etching amount of about 1 nm.

[0071] The sputtering etching of the aluminum plate, for example, in the case of a single plate, can be carried out under vacuum at a plasma power of, for example, 100 W to 1 kW for 1 to 50 minutes; in the case of a long material such as a wire, it can be carried out under vacuum at a plasma power of, for example, 100 W to 10 kW and a line speed of 1 m / min to 30 m / min. The vacuum degree at this time is preferably a high vacuum degree to prevent the adsorbate from being adsorbed to the surface again, for example, 1×10 -5 The temperature of the aluminum plate is preferably kept at room temperature to 150° C. In the sputtering etching process, the room temperature refers to 15° C. to 25° C.

[0072] The sputtering etching process of the copper plate, for example, in the case of a single plate, can be carried out under vacuum at a plasma power of, for example, 100 W to 1 kW for 1 to 50 minutes; in the case of a long material such as a wire, it can be carried out at a plasma power of 100 W to 10 kW and a line speed of 1 m / min to 30 m / min. The vacuum degree at this time is preferably a high vacuum degree to prevent the adsorbate from being adsorbed to the surface again, 1×10 -5 The temperature may be Pa to 10 Pa. During the sputtering etching process, the temperature of the copper plate is preferably maintained at room temperature to 150°C.

[0073] Next, the sputter-etched surfaces (joining surfaces) of the aluminum plate and the copper plate are pressed together, for example by roller pressing, so that the reduction rate of the rolled joint body reaches more than 3%, thereby joining the aluminum plate and the copper plate (joining step).

[0074] The reduction rate of the rolled joint body is 3% or more, preferably 4% or more, more preferably 4.5% or more, and particularly preferably 5% or more. When the reduction rate of the rolled joint body is 3% or more, a rolled joint body with sufficiently high peel strength can be obtained. The upper limit of the reduction rate of the rolled joint body is generally 10% or less. From the viewpoints of shape control and hardness, it is preferably 8% or less, and particularly preferably 6% or less. The reduction rate of the rolled joint body is preferably 3% to 10%, more preferably 3% to 8%, and particularly preferably 3% to 6%. The reduction rate of the rolled joint body is calculated according to the total thickness of the aluminum plate and the copper plate before joining and the thickness of the final rolled joint body by the following formula: (total thickness of the aluminum plate and the copper plate before joining-thickness of the final rolled joint body) / total thickness of the aluminum plate and the copper plate before joining.

[0075] There is no particular restriction on the calender line load of the roller crimping, and it can be set to achieve the specified reduction rate of the rolled joint body, for example, it can be set to the range of 0.1tf / cm to 10.0tf / cm. For example, when the roller diameter of the crimping roller is 300mm to 400mm, the calender line load of the roller crimping is preferably 0.1tf / cm to 3.0tf / cm, more preferably 0.3tf / cm to 3.0tf / cm, and particularly preferably 0.3tf / cm to 1.8tf / cm. Among them, in the case where the roller diameter becomes larger and the thickness of the aluminum plate and the copper plate before joining is thicker, in order to achieve the specified reduction rate, it is sometimes necessary to increase the calender line load to ensure the pressure, and it is not limited to this numerical range.

[0076] The temperature during bonding is not particularly limited, and is, for example, room temperature to 150°C.

[0077] The bonding is preferably performed in a non-oxidizing atmosphere, for example, an inert gas atmosphere such as Ar, to prevent the surfaces of the aluminum plate and the copper plate from re-adsorbing oxygen and causing a decrease in the bonding strength between the two.

[0078] In the manufacturing method of the present invention, the rolled joint body obtained by joining the aluminum plate and the copper plate as above is not subjected to heat treatment, or is subjected to heat treatment at a temperature below 250°C, preferably below 220°C. By controlling the heat treatment in this way, the formation of intermetallic compounds can be suppressed, so that the rolled joint body has high peel strength and high resistance to bonding and bending. Whether to use heat treatment can be selected according to the purpose of the rolled joint body. For example, when heat treatment is performed below 220°C, the peel strength of the rolled joint body can be further improved, and the copper layer can also be softened. In particular, by softening the copper layer, the hardness ratio of the aluminum layer and the copper layer can be controlled within the above range, for example, it can be suitable for uses such as wires that require flexibility.

[0079] When heat treatment is performed, the heat treatment temperature is lower than 250°C, preferably lower than 220°C. Setting the heat treatment temperature to 220°C or lower can inhibit the formation of intermetallic compounds. From the viewpoint of being able to obtain sufficiently high peel strength, the lower limit of the heat treatment temperature is preferably 100°C or higher, more preferably 150°C or higher. The heat treatment temperature is preferably 100°C to 220°C, more preferably 150°C to 220°C.

[0080] The heat treatment time can be appropriately set according to the heat treatment temperature or the size of the rolled joint body to be heat treated to prevent the formation of intermetallic compounds. The heat treatment time is, for example, 0.5 hours to 8 hours, preferably 0.5 hours to 5 hours, and particularly preferably 0.5 hours to 3 hours. It should be noted that if intermetallic compounds are not generated, there is no problem with heat treatment for more than 8 hours. In addition, the heat treatment time refers to the time after the rolled joint body to be heat treated reaches the specified temperature, and does not include the heating time of the rolled joint body. For example, if the heat treatment temperature is 150°C, the heat treatment time is generally 0.5 hours to 8 hours; if the heat treatment temperature is 200°C, the heat treatment time is generally 0.5 hours to 5 hours; if the heat treatment temperature is 220°C, the heat treatment time is generally 0.5 hours to 3 hours.

[0081] The rolled joint body of the present invention has no intermetallic compounds at the interface and has a sufficiently high peel strength, so it has high resistance to bonding and bending processing, and can suppress the generation of cracks and peeling even in bending processing under more severe conditions, so that it can be applied to bonding wires, bonding tapes, and wires. Therefore, the present invention also includes bonding wires, bonding tapes, and wires composed of the above-mentioned rolled joint body. The bonding wires, bonding tapes, and wires of the present invention can be used in power modules, for example.

[0082] [Example]

[0083] The present invention is further described in detail below based on embodiments and comparative examples, but the present invention is not limited to these embodiments.

[0084] Example 1

[0085] The aluminum plate used was A1N30 (thickness 0.05 mm) with a hardness of HV 24.5, and the copper plate used was C1020 (thickness 0.15 mm) with a hardness of HV 122.5. The aluminum plate and the copper plate were bonded by a surface activation bonding method as follows to produce a rolled bonded body consisting of an aluminum layer and a copper layer.

[0086] Sputter etching was performed on each surface where A1N30 and C1020 were bonded. The sputter etching of A1N30 was performed by flowing Ar as the sputtering gas, at 0.2 Pa, with a plasma power of 300 W, for 1 minute; the sputter etching of C1020 was performed by flowing Ar as the sputtering gas, at 0.2 Pa, with a plasma power of 600 W, for 1 minute.

[0087] The sputtered and etched AlN30 and C1020 were joined by roll pressing at room temperature with a rolling roll diameter of 300 mm to 400 mm and a rolling line load of 0.9 tf / cm to 1.8 tf / cm to obtain a rolled joint body consisting of an aluminum layer and a copper layer. The rolling reduction of the rolled joint body was 5%.

[0088] Example 2

[0089] The rolled bonded body produced in the same manner as in Example 1 was heat treated at 220° C. for 1 hour to produce a rolled bonded body of Example 2.

[0090] Example 3

[0091] The rolled bonded body of Example 3 was produced in the same manner as in Example 1 except that A1050 (thickness 0.1 mm) with a hardness HV of 23.6 was used as the aluminum plate and C1020 (thickness 0.1 mm) with a hardness HV of 123.5 was used as the copper plate. The rolling reduction of the rolled bonded body was 3%.

[0092] Example 4

[0093] The rolled bonded body of Example 4 was produced in the same manner as in Example 3 except that A1050 (thickness 0.1 mm) having a hardness HV of 34.5 was used as the aluminum plate. The rolling reduction of the rolled bonded body was 3%.

[0094] Comparative Example 1

[0095] A rolled bonded body of Comparative Example 1 was produced in the same manner as in Example 2 except that the heat treatment conditions were changed to 400° C. and 3 hours.

[0096] Comparative Example 2

[0097] The rolled bonded body produced in the same manner as in Example 4 was heat treated at 350° C. for 1 hour to produce a rolled bonded body of Comparative Example 2.

[0098] Comparative Example 3

[0099] A rolled joined body of Comparative Example 3 was produced in the same manner as in Example 4 except that the pressing force during joining was changed and the reduction ratio of the rolled joined body was set to 2.5%.

[0100] Comparative Example 4

[0101] A rolled bonded body of Comparative Example 4 was produced in the same manner as in Example 2 except that the heat treatment conditions were changed to 250° C. and 1 hour.

[0102] The following properties were measured for the rolled joined bodies of Examples 1 to 4 and Comparative Examples 1 to 4.

[0103] [hardness]

[0104] The hardness was measured using a micro Vickers hardness tester in accordance with JIS Z 2244 (Vickers hardness test - test method).

[0105] [Surface roughness Ra, Rz]

[0106] The surface roughness Ra and Rz of the aluminum layer and the copper layer of the rolled joint body were measured using a three-dimensional surface roughness profile measuring instrument (SURFCOM 1400D-3DF manufactured by Tokyo Seimitsu Co., Ltd.) in accordance with JIS-B0601-1994.

[0107] [Peel strength]

[0108] A test piece with a width of 20 mm was made from the rolled joint. After the aluminum layer and the copper layer were partially peeled off, the copper layer side was fixed and the force (unit: N / cm) required for peeling when the aluminum layer was pulled 180° to the opposite side of the copper layer at a tensile speed of 20 mm / min was measured using a TENSILON universal material testing machine RTC-1350A (manufactured by ORIENTEC Co., Ltd.).

[0109] [Confirm the presence or absence of intermetallic compounds]

[0110] After the rolled joint body was cross-sectioned by an ion cross-section polisher (CP), the cross section was observed at 2000 times using a scanning electron microscope (SEM) to confirm whether there was an intermetallic compound. In Table 1, the presence of an intermetallic compound with a thickness of 0.1 μm or more at the interface between the aluminum layer and the copper layer was recorded as "yes", and the absence of an intermetallic compound with a thickness of 0.1 μm or more was recorded as "no".

[0111] [Check whether there are cracks caused by bending and rebending]

[0112] A test piece of 50 mm long and 10 mm wide was made from the rolled joint body, and then the obtained test piece was clamped and fixed with a clamp, and then bent to 90° and then restored. After the cross section of the processed rolled joint body was manually polished, the cross section was observed at 2000 times using a scanning electron microscope (SEM) to confirm whether there were cracks. In Table 1, the presence of cracks was recorded as "yes", and the absence of cracks was recorded as "no".

[0113] [Bending peel test]

[0114] A test piece of 50 mm long and 10 mm wide was made from the rolled joint, bent 90° using a bending tester, and then bent 90° to the opposite side. This step was repeated until the test piece broke, and whether there was peeling of the layer after the test piece broke was confirmed. In Table 1, the case of peeling was recorded as "yes", and the case of no peeling was recorded as "no". In addition, Table 2 shows the number of bends until the test piece broke.

[0115] Regarding the rolled joints of Examples 1 to 4 and Comparative Examples 1 to 4, the characteristics of the original plates and the evaluation results of the rolled joints are shown in the following Table 1. In addition, Figures 1A to 1D show the results of confirming whether intermetallic compounds exist. Figure 1A is a cross-sectional SEM image of the rolled joint of Example 1 (2000 times); Figure 1B is a cross-sectional SEM image of the rolled joint of Example 2 (2000 times); Figure 1C is a cross-sectional SEM image of the rolled joint of Comparative Example 1 (2000 times); Figure 1D is a cross-sectional SEM image of the rolled joint of Comparative Example 4 (2000 times). In addition, Figure 2 A to C show the results of confirming the presence or absence of cracks caused by bending and rebending. Figure 2 A is a cross-sectional SEM image (2000 times) of the rolled joint body of Example 1; Figure 2 B is a cross-sectional SEM image (2000 times) of the rolled joint body of Example 2; Figure 2 C is a cross-sectional SEM image of the rolled bonded body of Comparative Example 1 (magnification 2000).

[0116]

Table 1

[0117]

[0118] As shown in Table 1, the rolled joints of Examples 1 to 4 have no intermetallic compounds at the interface, and the peel strength exceeds 10 N / cm, showing high resistance to bending and folding. Comparison of Examples 1 and 2 with Comparative Examples 1 and 4 shows that when heat treated at a temperature above 250°C, intermetallic compounds are generated at the interface (see Figures 1A to 1D), and cracks are generated at the interface during bending and folding (see Figures 1A to 1D). Figure 2 A to C), peeling occurs during bending, and the resistance to bending and bending processing is reduced. In addition, regarding the use of other aluminum, the comparison between Example 4 and Comparative Example 2 shows that when heat treatment is performed at 350°C, intermetallic compounds are generated, and the resistance to bending and bending processing is reduced; the comparison between Example 4 and Comparative Example 3 shows that when the reduction rate of the rolled joint body is low, a sufficiently high peeling strength cannot be obtained.

[0119] Table 2 below shows the hardness and hardness ratio of each layer of the rolled bonded bodies of Examples 1 to 4 and Comparative Example 1, and the number of bends required until the test piece broke in the bending peel test.

[0120]

Table 2

[0121]

[0122] As shown in Table 2, in the rolled joints of Examples 1 to 4 without intermetallic compounds at the interface, the closer the hardness ratio (Cu layer / Al layer) of the copper layer to the aluminum layer is to 1, the more they can withstand more severe bending processing. This is because, when the hardness difference between the copper layer and the aluminum layer is large, cracks tend to spread from the location where the cracks occur. The closer the hardness ratio is to 1, the more the hardness of the two layers will be balanced, thereby suppressing the spread of cracks. On the other hand, in the rolled joint of Comparative Example 1 with intermetallic compounds at the interface, although the hardness ratio is close to 1, it breaks earlier than the rolled joints of Examples 1 to 4. This is because the rolled joint of Comparative Example 1 has intermetallic compounds at the interface, so cracks occur early, and then the cracks propagate to the aluminum layer and the copper layer until they break. In addition, as shown in Table 2, the rolled joint of Example 2 was heat treated at 220°C, so that compared with Example 1 that was not heat treated, the hardness of the aluminum layer was the same and the hardness of the copper layer was greatly reduced.

[0123] All publications, patents and patent applications cited in this specification are incorporated into this specification by direct reference.

Claims

1. A rolled joint body, comprising an aluminum layer and a copper layer, wherein an intermetallic compound containing aluminum and copper does not exist at an interface between the aluminum layer and the copper layer, and wherein a peel strength exceeds 10 N / cm.

2. The rolled bonded body according to claim 1, wherein: The aluminum layer has a hardness HV of 40 or less.

3. The rolled bonded body according to claim 1 or 2, wherein: The surface roughness Rz of the aluminum layer is 0.5 μm or less.

4. The rolled bonded body according to any one of claims 1 to 3, wherein Aluminum is 1000 series pure aluminum specified in JIS.

5. The rolled joined body according to any one of claims 1 to 4, wherein The copper layer has a hardness HV of 130 or less.

6. The rolled joined body according to any one of claims 1 to 5, wherein The copper is 1000 series pure copper specified in JIS.

7. The rolled joined body according to any one of claims 1 to 6, wherein The ratio of the hardness of the copper layer to the hardness of the aluminum layer (hardness of the copper layer / hardness of the aluminum layer) is 1.0 to 5.

0.

8. The rolled joined body according to any one of claims 1 to 7, wherein The rolled joint body is in a linear or strip shape.

9. A method for manufacturing a rolled bonded body, wherein the rolled bonded body is the rolled bonded body according to any one of claims 1 to 8, the method comprising the following steps: Sputter etching of aluminum plates; Sputter etching of copper plates; as well as, The surfaces of the aluminum plate and the copper plate after sputtering etching are press-bonded to each other so that the rolling reduction rate of the rolled joint body reaches 3% or more, After the step of joining, a heat treatment below 250° C. is performed, or no heat treatment is performed. 10 . A bonding wire or a bonding ribbon, comprising the rolled bonded body according to claim 1 .