Method for purifying lignin
By immersing lignin in an acidic aqueous solution, the problem of removing metallic impurities from lignin in existing technologies is solved, achieving efficient and low-cost lignin purification, making it suitable for carbon enrichment materials in energy storage applications.
Patent Information
- Application Number
- CN202380029837.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-04
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-15
AI Technical Summary
Existing technologies struggle to efficiently and cost-effectively remove metallic impurities, particularly transition metals such as iron and manganese, from lignin, leading to stability issues in energy storage applications.
The lignin is immersed in an acidic aqueous solution at 40°C to 100°C for more than 15 minutes, then separated and optionally washed. Organic acids such as oxalic acid or formic acid are used to reduce the metal content, keeping the lignin in solid form.
It achieves efficient purification of lignin, reducing the total metal content to below 200 ppm, making it suitable for carbon enrichment materials in energy storage applications, simplifying process steps and reducing costs.
Smart Images

Figure BDA0005056641140000111 
Figure BDA0005056641140000112 
Figure BDA0005056641140000113
Abstract
Description
Technical Field
[0001] The present invention relates to a method for purifying lignin, wherein metals are removed from the lignin. In addition, the present invention relates to lignin with a total metal content below 200 ppm. The purified lignin can be further processed into end products such as carbon-enriched materials. Background Art
[0002] Lignin (an aromatic polymer) is the main component of wood, for example, and is the most abundant source of carbon on Earth after cellulose. In recent years, with the development and commercialization of technologies to extract highly purified, solid and particularized forms of lignin from pulping processes, it has attracted great attention as a possible renewable alternative to the main aromatic chemical precursors currently derived from the petrochemical industry.
[0003] Nowadays, the most commercially relevant source of lignin is kraft lignin. This lignin is obtained from hardwood or softwood by the kraft process. The lignin can be separated from alkaline black liquor using, for example, membrane filtration or ultrafiltration. LignoBoost is a conventional separation process and is described in, for example, WO2006031175 A1. In this process, lignin is precipitated from alkaline black liquor by reducing the pH level (usually by adding carbon dioxide) and then filtered out. In the next step, the lignin filter cake is re-pulped (usually using sulfuric acid) and washed under acidic conditions. The precipitated washed lignin can be used directly or further dried.
[0004] Black liquor is readily available as a byproduct from the kraft process and is thus a cost-effective source of lignin. However, since black liquor contains a certain amount of metals, mostly derived from wood and from the cooking chemicals used during the pulping process, the lignin precipitated from the black liquor will also contain a certain amount of metals. Typically, lignin will contain relatively high levels of sodium and potassium and lower amounts of other metals such as aluminum, calcium, iron, magnesium and manganese. Lignin may also contain trace amounts of other metals.
[0005] During the separation process, some metals (such as sodium and potassium) can be removed from the precipitated lignin to a large extent by an acidic washing step. However, it is more difficult to remove other metals from the precipitated lignin. In many potential applications, such as in biofuels and for the conversion of materials (such as carbon fibers and carbon powder) to carbon enrichment, it is important that the lignin used has high purity, particularly relative to the amount of metal, otherwise it can interfere with the functionality of the material. When lignin is further intended to be used for the conversion of materials to carbon enrichment (the material is then used in energy storage applications), this is particularly important. Specifically, if present in energy storage applications involving materials of carbon enrichment obtained from lignin, transition metals such as iron and manganese can have a negative impact on the long-term stability of energy storage devices. It is believed that this is caused by the precipitation of transition metals during charging and discharging, and also by the decomposition of the electrolyte reacted by catalysis via transition metals.
[0006] Lignin can also be obtained by different fractionation methods such as organosolv process or hydrolysis of lignin.However, the commercial interest of organosolv process for producing lignin is lower compared to kraft process.
[0007] Various attempts to remove metals from lignin have been made. Common to these methods is that they are quite complex, involving many additional processing steps; and / or they are not sufficiently efficient in their metal removal efficiency, resulting in insufficient purity levels and / or long washing times.
[0008] KR101451299 B1 discloses a method in which lignin is repeatedly dissolved and precipitated to obtain lignin with a low ash content. However, many additional process steps are required.
[0009] WO2020013752 A1 discloses a method for dissolving lignin in an acidic aqueous solvent. A two-phase system is obtained by phase separation, in which one phase is a lignin-rich phase and the other phase lacks lignin and contains metal cations extracted from lignin. However, many additional process steps are required.
[0010] Thus, there is a need for an improved method for purifying lignin, wherein the purified lignin obtained has a sufficiently low metal content so that the purified lignin can also be used in applications requiring high-purity materials. In addition, the method should be cost-effective and compatible with large-scale production. Summary of the invention
[0011] It is an object of the present invention to provide an improved process for purifying lignin which obviates or mitigates at least some of the disadvantages of prior art processes.
[0012] It is a further object of the present invention to provide a process for purifying lignin, wherein the lignin obtained has a reduced total metal content.
[0013] It is a further object of the present invention to provide a method for purifying lignin which is compatible with large-scale production.
[0014] The above-mentioned objects and other objects that those skilled in the art will appreciate based on the present invention are achieved through various aspects of the present invention.
[0015] According to a first aspect, the present invention relates to a method for purifying lignin, wherein the method comprises the following steps:
[0016] a) providing lignin in solid form;
[0017] b) providing an acidic aqueous solution having a pH below 6;
[0018] c) immersing the lignin in the acidic aqueous solution for at least 15 minutes, wherein the temperature of the acidic aqueous solution during immersion is in the range of from 40° C. to 100° C., to remove metals from the lignin to the acidic aqueous solution, so as to obtain the purified lignin;
[0019] d) separating the obtained purified lignin from the acidic aqueous solution; and
[0020] e) optionally washing the separated purified lignin
[0021] Therein the lignin remains in solid form during all steps of the process.
[0022] The method of the invention according to the first aspect is based on the surprising recognition that metals can be removed from lignin in solid form by immersing the lignin in an acidic aqueous solution at a temperature in the range from 40° C. to 100° C. for at least 15 minutes. This enables a method for purifying lignin which is fast and comprises few additional method steps and which can be carried out using existing processing equipment employed during the production of lignin from black liquor. The method is thus compatible with large-scale production.
[0023] According to a second aspect, the present invention relates to lignin having a total metal content below or equal to 200 ppm.
[0024] Lignin materials with low metal contents are of interest in a number of different applications, such as in biofuels and for conversion to carbon-rich materials such as carbon fibers and carbon powders, particularly for use in energy storage applications. DETAILED DESCRIPTION
[0025] Step a) of the method according to the first aspect involves providing lignin in solid form. Throughout this specification, the expression "lignin" is intended to cover any kind of lignin, such as lignin derived from hardwood, softwood or annular plants. Lignin may also be chemically modified. Preferably, the lignin has been purified or separated before being used in the process according to the present invention. Lignin may be separated from black liquor and optionally further purified before being used in the process according to the present invention. Purification typically results in a purity of the lignin material of at least 90%, preferably at least 95%, more preferably at least 98%, based on the dry weight of the lignin material. Thus, the lignin material used in the process according to the present invention preferably contains less than 10%, preferably less than 5%, more preferably less than 2% impurities, such as cellulose and inorganic compounds, based on the dry weight of the lignin material.
[0026] Lignin can be obtained by different fractionation methods such as an organosolv process or a kraft process. Preferably, the lignin provided in step a) of the method according to the first aspect is kraft lignin, i.e. lignin obtained by a kraft process. Preferably, the kraft lignin is obtained from hardwood or softwood, most preferably from softwood.
[0027] Lignin can be obtained by using a process commonly referred to as the LignoBoost process disclosed in WO2006031175 A1. Typically, the process involves the steps of precipitation of lignin from alkaline black liquor by acidification; separation of the precipitated lignin; and re-slurrying the lignin at least once under acidic conditions. The obtained lignin can be dried and pulverized and thus provided as solid particles. The lignin obtained by this method typically has a total metal content in the range of from 500ppm to 5000ppm, mainly derived from wood sources and cooking chemicals added during the pulping process. The pH of the obtained lignin is typically in the range of from 3 to 4. The sulfur content of the obtained lignin is typically about 1-3% by weight. This lignin is a preferred starting material for the method of the present invention.
[0028] As used herein, the term "total metal content" refers to the total amount of metals present in lignin. Typically, the metals present in lignin are sodium, potassium, magnesium, calcium, aluminum, iron and manganese. Other metals may also be present in trace amounts. The metal content can be determined by inorganic element analysis. The total metal content is determined by summing up the amounts of all individual metals. In one embodiment, the lignin provided in the step a) of the method of the present invention according to the first aspect has a total metal content of at least 500ppm, preferably at least 600ppm and more preferably at least 700ppm. In another embodiment, the lignin provided in the step a) of the method according to the first aspect has a total metal content in the range from 500ppm to 5000ppm, preferably in the range from 600ppm to 3000ppm and more preferably in the range from 700ppm to 1500ppm.
[0029] In one embodiment, the lignin provided in step a) of the method according to the first aspect may have an aluminum content of at least 18 ppm or at least 19 ppm; a calcium content of at least 18 ppm or at least 19 ppm; an iron content of at least 16 ppm or at least 17 ppm; a potassium content of at least 30 ppm or at least 50 ppm; a magnesium content of at least 45 ppm or at least 48 ppm; a manganese content of at least 11 ppm or at least 12 ppm; and a sodium content of at least 400 ppm or at least 650 ppm.
[0030] In an alternative embodiment, the lignin provided in step a) of the method according to the first aspect has an aluminum content in the range of from 18 to 25 ppm, preferably from 19 to 23 ppm; a calcium content in the range of from 18 to 40 ppm, preferably from 19 to 25 ppm; an iron content in the range of from 16 to 30 ppm, preferably from 17 to 22 ppm; a potassium content in the range of from 30 to 90 ppm, preferably from 50 to 70 ppm; a magnesium content in the range of from 45 to 55 ppm, preferably from 48 to 53 ppm; a manganese content in the range of from 11 to 30 ppm, preferably from 12 to 16 ppm; and a sodium content in the range of from 400 ppm to 2000 ppm, preferably from 650 to 1000 ppm.
[0031] The lignin provided in step a) of the method according to the first aspect may further have a silicon content of at least 90 ppm, or at least 100 ppm. Alternatively, the silicon content may be in the range of from 90 to 140 ppm, preferably from 100 to 130 ppm.
[0032] The lignin provided in step a) of the method according to the first aspect is in solid form, i.e. it is not in a dissolved state. In one embodiment, the lignin is provided in the form of a dry powder. Alternatively, the lignin can be wet or provided in a slurry or suspension. The lignin can also be provided as a crushed lignin cake obtained from a lignin separation process. During any step in the method according to the first aspect, the lignin does not dissolve, but remains in solid form.
[0033] Alternatively, during the steps of the method according to the invention, the lignin may be dissolved to a small extent, so that only small fragments of solid lignin are dissolved. Thus, the lignin will remain mainly in a solid state. Any dissolved lignin will be removed during the separation step and discarded from the process.
[0034] Preferably, the lignin provided in step a) of the method according to the first aspect is in the form of particles, such as in the form of a powder. The particle size distribution of the lignin particles is preferably such that at least 80% by weight of the particles have a diameter of less than 0.2 mm. In the context of the present invention, if the particles are not spherical, the diameter of the particles is the equivalent spherical diameter of the particles. The equivalent spherical diameter is the diameter of a sphere of equivalent volume.
[0035] Step b) of the method according to the first aspect involves providing an acidic aqueous solution having a pH below 6. The term "acidic aqueous solution" as used herein refers to any type of aqueous solution having a pH below 7. The acidic aqueous solution in step b) of the method according to the first aspect can be provided by adding at least one acid to the aqueous solution. The pH of the acidic aqueous solution provided in step b) of the method according to the first aspect has a pH below 6, preferably below 5 and more preferably below 4. In an alternative embodiment, the pH of the acidic aqueous solution may be below 7. In yet another alternative embodiment, the pH of the acidic aqueous solution may be in the range from 1 to 6, preferably from 1 to 5, and more preferably from 1 to 4.
[0036] Lignin can be added to the aqueous solution after the acid has been added. Alternatively, lignin can be added to the aqueous solution before the acid is added. Or the aqueous solution is heated before the addition of acid and lignin or after the addition of acid and lignin. In one embodiment, acid is added to the heated aqueous solution and lignin is subsequently added to the heated aqueous solution. In another embodiment, lignin is added to the acidic aqueous solution and then heated. In yet another embodiment, acid is added to the aqueous solution containing lignin. In this embodiment, the aqueous solution is heated before or after the addition of acid. In a preferred embodiment, lignin is added to the heated aqueous solution and acid is subsequently added to the aqueous solution containing lignin.
[0037] The acidic aqueous solution comprises at least one acid such that the pH of the acidic aqueous solution is below 7, or below 6, or below 5, or below 4. In a preferred embodiment, the acidic aqueous solution comprises at least one organic acid. The organic acid may be a carboxylic acid and may be monoprotic, diprotic, or triprotic. In a preferred embodiment, the organic acid has a pKa value equal to or less than 4.75 for at least one acidic group. The organic acid may be selected from at least one of acetic acid, citric acid, formic acid, and oxalic acid. Preferably, the acidic aqueous solution comprises at least one organic acid selected from formic acid and oxalic acid. It has been found that the use of organic acids further reduces the metal content in lignin during the immersion step. Compared with acids containing sulfur, nitrogen, and / or phosphorus, organic acids such as formic acid and oxalic acid are cheap, easy to handle, have low toxicity, and are generally less subject to certain waste disposal regulations.
[0038] In alternative embodiments, the acidic aqueous solution comprises at least one inorganic acid such as sulfuric acid, hydrochloric acid, or phosphoric acid.
[0039] The acidic aqueous solution may also contain more than one acid, such as a combination of two or more organic acids or inorganic acids. The acidic aqueous solution may also contain a combination of organic acids and inorganic acids. In one embodiment, the acidic aqueous solution contains both formic acid and oxalic acid.
[0040] In one embodiment of the method according to the first aspect, the total amount of acid in the acidic aqueous solution is in the range of from 0.1 to 6 weight %, preferably from 0.5 to 5 weight %, based on the dry weight of lignin immersed in the acidic aqueous solution. As used herein, the term "total amount of acid" refers to the total amount of concentrated acid added to the acidic aqueous solution. Increasing the amount of acid can increase the removal of metal from lignin. However, it is beneficial to avoid using a large amount of acid from the perspective of technology, for cost reasons and because it is conducive to waste treatment. By increasing the amount of acid in the acidic aqueous solution, the side reaction of degradable lignin can also be triggered.
[0041] The acidic aqueous solution may further comprise one or more additives. The additive may be a dispersant, such as glycerol or a fatty acid. The additive may also be an oxidant such as hydrogen peroxide or EDTA. Other additives include ion exchangers such as ammonium salts such as ammonium acetate and ammonium sulfate. The additives in the acidic aqueous solution may enhance the effect of removing metals from lignin.
[0042] Step c) of the method according to the first aspect involves immersing the lignin particles in an acidic aqueous solution for at least 15 minutes, wherein the temperature of the acidic aqueous solution during the immersion is in the range from 40°C to 100°C, so as to remove metals from the lignin into the acidic aqueous solution so as to obtain said purified lignin.
[0043] The term "immersion" as used herein refers to a process in which lignin in solid form (such as in the form of lignin particles) is contacted with an acidic aqueous solution for a certain period of time. During the immersion step of the method according to the first aspect, the entire surface area of the lignin is contacted with the acidic aqueous solution, meaning that the lignin is completely immersed in the acidic aqueous solution.
[0044] Lignin is immersed in an acidic aqueous solution at a temperature in the range of from 40°C to 100°C, such as from 50°C to 90°C or from 60°C to 80°C. In one embodiment, lignin is immersed in an acidic aqueous solution at a temperature in the range of from 40°C to 110°C, such as from 80°C to 100°C. The acidic aqueous solution can be heated in any suitable manner known to those skilled in the art. The temperature is maintained in a defined range during the entire immersion step. The metal removal efficiency is improved by heating the acidic aqueous solution. However, if too high a temperature is used, the lignin may be damaged or degraded.
[0045] According to the step c) of the method of the first aspect, the immersion time is at least 15 minutes, preferably at least 30 minutes, or more preferably at least 1 hour. In an alternative embodiment of the method according to the first aspect, the immersion time is in the range of from 15 minutes to 6 hours, preferably in the range of from 30 minutes to 5 hours, or even more preferably in the range of from 1 hour to 4 hours. The metal removal efficiency can be improved by increasing the immersion time. However, in order to be able to realize a cost-effective method that can be easily scaled up, it is important to have a relatively short immersion time. However, the immersion time must be long enough for fully removing metals from lignin.
[0046] In a preferred embodiment of the method according to the first aspect, the acidic aqueous solution is stirred during the immersing step.Any suitable stirring means as known to those skilled in the art may be used.
[0047] During the immersion step, metals are removed from the lignin to the acidic aqueous solution so that purified lignin is obtained. As used herein, the term "purified lignin" refers to a lignin material that essentially only comprises lignin, such as at least 99% by weight of lignin based on the dry weight of the lignin material and other components such as cellulose and inorganic compounds that are less than 1% by weight based on the dry weight of the lignin material. In particular, the purified lignin comprises a reduced amount of metal. In a preferred embodiment of the method according to the first aspect, the purified lignin obtained in the step c) of the method has a total metal content of less than 200ppm, preferably less than 150ppm and more preferably less than 100ppm. As mentioned above, lignin is not dissolved during the immersion step, which means that metals are removed from solid lignin and not removed from dissolved lignin. Thus, the purified lignin obtained in the step c) of the method according to the first aspect is also in solid form, such as in the form of particles.
[0048] Low-metal lignin is obtained by the method of the invention according to the first aspect. Preferably the lignin is in the form of particles so that low-metal lignin particles are obtained.
[0049] Step d) of the method according to the first aspect involves separating the purified lignin obtained from the acidic aqueous solution. The purified lignin is in solid form during separation. The term "separation" as used herein refers to a process of separating lignin from an acidic aqueous solution.
[0050] In a preferred embodiment of the method according to the first aspect, the separation in step d) is carried out using filtration. Alternatively, the separation can be carried out by centrifugation or sedimentation or any other suitable means known to those skilled in the art. Since the purified lignin is separated from the acidic aqueous solution, the pH of the acidic aqueous solution and the lignin during the separation step will be the same as the pH during the immersion step. Thus, during the step of separating the purified lignin, the pH of the aqueous acidic solution is below 6, preferably below 5, or more preferably below 4. In one embodiment, the pH of the aqueous acidic solution can be in the range of from 1 to 7, preferably from 2 to 6, more preferably from 2 to 5, and most preferably from 2 to 4.
[0051] In one embodiment of the method according to the first aspect, steps cd and optionally e) are repeated at least once. In this embodiment, before the second separation step, the separated lignin is immersed in an acidic aqueous solution for the second time. The pH, temperature and time of the acidic aqueous solution during the immersion step are selected as discussed above. In an embodiment of repeated immersion and separation steps, parameters such as pH, temperature and time during immersion may be the same as all immersion steps or they may change between different immersion steps. In one embodiment, the same parameters are used during two immersion steps. In one embodiment, the pH in the second immersion step may be lower than the pH in the first immersion step. In another embodiment, the immersion time in the second immersion step may be shorter than the immersion time in the first immersion step. In yet another embodiment, the temperature in the first immersion step may be higher than the temperature in the second immersion step. The total immersion time is the sum of the immersion times for a single step. Separation is preferably carried out by filtration after each immersion step. By adding additional immersion steps and by optimizing the parameters of each step such as time, temperature and pH, the metal content of lignin can be further reduced.
[0052] Step e) of the method according to the first aspect involves optionally washing the separated purified lignin. In one embodiment of the method according to the first aspect, the separated lignin is subjected to washing with an aqueous washing solution. The aqueous washing solution is preferably water. In one embodiment, the separated purified lignin is washed with water until the pH of the water used for washing becomes neutral.
[0053] In one embodiment of the method according to the first aspect, the method comprises an additional step of drying the separated and optionally washed purified lignin. The purified lignin can be dried after the separation step or after the optional washing step. The drying of the purified lignin can be carried out by methods and equipment known in the art. The temperature during drying is preferably in the range of from 60°C to 160°C, more preferably in the range of from 100°C to 120°C. Drying can be carried out under ambient pressure, reduced pressure or vacuum.
[0054] The purified lignin obtained by the method according to the first aspect may have a total metal content of less than 200 ppm, preferably less than 150 ppm and more preferably less than 100 ppm.
[0055] The purified lignin obtained by the method according to the first aspect may have an aluminum content of less than 17 ppm, or less than 13 ppm; a calcium content of less than 16 ppm, or less than 10 ppm; a potassium content of less than 10 ppm, or less than 5 ppm; a magnesium content of less than 42 ppm, or less than 25 ppm; and a sodium content of less than 30 ppm, or less than 15 ppm.
[0056] The purified lignin obtained by the method according to the first aspect may have an iron content of less than 15 ppm, preferably less than 10 ppm.
[0057] The purified lignin obtained by the method according to the first aspect may have a manganese content of less than 10 ppm, preferably less than 6 ppm.
[0058] In alternative embodiments, the purified lignin obtained by the method according to the first aspect may have a total metal content in the range from 0 to 200 ppm, such as from 0.1 to 200 ppm, preferably from 0 to 150 ppm, such as from 0.1 to 150 ppm, and more preferably from 0 to 100 ppm, such as from 0.1 to 100 ppm.
[0059] In alternative embodiments, the purified lignin obtained by the method according to the first aspect may have an iron content in the range from 0 to 15 ppm, or from 0 to 10 ppm, or from 0.1 to 15 ppm, or from 0.1 to 10 ppm.
[0060] In alternative embodiments, the purified lignin obtained by the method according to the first aspect may have a manganese content in the range from 0 to 10 ppm, or from 0 to 6 ppm, or from 0.1 to 10 ppm, or from 0.1 to 6 ppm.
[0061] In alternative embodiments, the purified lignin obtained by the method according to the first aspect may have an aluminum content in the range of from 0 to 17 ppm, or from 0 to 13 ppm; a calcium content in the range of from 0 to 16 ppm, or from 0 to 10 ppm; a potassium content in the range of from 0 to 10 ppm, or from 0 to 5 ppm; a magnesium content in the range of from 0 to 42 ppm, or from 0 to 25 ppm; and a sodium content in the range of from 0 to 30 ppm, or from 0 to 15 ppm.
[0062] In alternative embodiments, the purified lignin obtained by the method according to the first aspect may have an aluminum content in the range of from 0.1 to 17 ppm, or from 0.1 to 13 ppm; a calcium content in the range of from 0.1 to 16 ppm, or from 0.1 to 10 ppm; a potassium content in the range of from 0.1 to 10 ppm, or from 0.1 to 5 ppm; a magnesium content in the range of from 0.1 to 42 ppm, or from 0.1 to 25 ppm; and a sodium content in the range of from 0.1 to 30 ppm, or from 0.1 to 15 ppm.
[0063] The lignin provided as starting material in step a) of the method according to the first aspect preferably has a metal content in the range of from 500 ppm to 5000 ppm. This means that the reduction in total metal content by the method of the present invention can be at least 60%, preferably at least 70%, and more preferably at least 80%.
[0064] During the immersion step, other inorganic impurities such as silicones may also be removed from the lignin into the acidic aqueous solution. Thus, in one embodiment of the method according to the first aspect, silicones are also removed from the lignin into the acidic aqueous solution during the immersion step; and the purified lignin obtained has a silicone content of less than 80 ppm, such as in the range of from 0 to 80 ppm, or from 0.1 to 80 ppm.
[0065] The purified lignin obtained by the method according to the first aspect may be subjected to further treatments, such as various thermal treatments.
[0066] The purified lignin obtained by the method according to the first aspect is particularly suitable for further conversion into carbon-enriched materials intended for energy storage applications and for other applications where lignin materials having a total metal content of less than 200 ppm are of interest.
[0067] The lignin according to the second aspect of the present invention has a total metal content of less than or equal to 200ppm. The lignin is obtained by the method according to the first aspect. Due to the low metal content of the lignin, it is suitable for further conversion to carbon-enriched materials in energy storage applications. The lignin according to the second aspect can be further limited as described above with respect to the first aspect.
[0068] Example
[0069] Kraft lignin powder obtained from the LignoBoost process was used in all examples.
[0070] The content of inorganic substances such as aluminum, calcium, iron, potassium, magnesium, manganese, sodium and silicone in lignin samples (i.e. lignin powders that have undergone various treatments) is evaluated by ICP-OES (Inductively Coupled Plasma-Optical Emission Spectrometry). The lignin samples are oxidized with hydrogen peroxide and then wet digested with nitric acid in a microwave oven. The content of inorganic substances is quantified by ICP-OES. The total metal content is calculated by summing up the content of individual metals.
[0071] The inorganic content of the lignin powder starting material (Sample 0) before any treatment was also evaluated by ICP analysis, see Table 1.
[0072] Table 1: Inorganic content in kraft lignin powder, “Metal” refers to the total metal content.
[0073]
[0074] Example 1 - Type of Acid
[0075] Kraft lignin powder (150 g) from the LignoBoost process was added to heated water (1.5 l, 60 ° C or 80 ° C) during stirring. After that, 7.5 g (5 wt %, based on the dry weight of lignin added to the water) of acid (oxalic acid, formic acid, phosphoric acid or sulfuric acid) was added and the mixture was stirred at a maintained temperature for a period of 4 hours. The mixture was then filtered and the lignin was collected and dried overnight in a vacuum oven at 60 ° C. The experimental details are summarized in Table 2 and the results from the ICP analysis are summarized in Table 3. It can be noted that oxalic acid at 80 ° C (1d) gave the highest lignin purity, while being the lowest total metal content and the lowest level of key transition metals such as Fe and Mn.
[0076] Table 2: Experimental details for Example 1
[0077]
[0078] Table 3: Inorganic content in samples from Example 1. "Metal" refers to the total metal content.
[0079]
[0080] Example 2 - Comparative Example
[0081] In the comparative example, kraft lignin powder (150 g) from the LignoBoost process was added to heated water (1.5 l) having a temperature of 60° C. (Sample 2a) or 80° C. (Sample 2b) during stirring. The mixture was stirred at the maintained temperature for a period of 4 hours. No acid was added. The mixture was then filtered and the lignin was collected and dried overnight in a vacuum oven at 60° C. The results from the ICP analysis are summarized in Table 4.
[0082] Table 4: Inorganic content of samples from Example 2. "Metal" refers to the total metal content.
[0083]
[0084] Example 3 - Amount of Acid Added
[0085] Kraft lignin powder (150 g) from the LignoBoost process was added to heated water (1.5 l, 60°C or 80°C) during stirring. After that, 1.5 g or 7.5 g (1 wt % or 5 wt %, respectively, based on the dry weight of lignin added to the water) of acid (oxalic acid or formic acid) was added and the mixture was stirred at the maintained temperature for a period of 4 hours. The mixture was then filtered and the lignin was collected and dried in a vacuum oven at 60°C overnight. The experimental details are summarized in Table 5 and the results from the ICP analysis are summarized in Table 6. It is evident that increasing the amount of acid from 1 wt % to 5 wt % has only a small effect when the wash is maintained at 60-80°C for four hours.
[0086] Table 5: Experimental details for Example 3
[0087]
[0088] Table 6: Inorganic content in samples from Example 3. "Metal" refers to the total metal content.
[0089]
[0090] Example 4 - Temperature of Acidic Aqueous Solution
[0091] Kraft lignin powder (150 g) from the LignoBoost process was added to water (1.5 l) during stirring. The water was heated to 20°C (sample 4a), 60°C (sample 4b) or 80°C (sample 4c). After that, 7.5 g (5 wt %, based on the dry weight of the lignin added to the water) of oxalic acid was added and the mixture was stirred at a maintained temperature for a period of 4 hours. The mixture was then filtered and the lignin was collected and dried overnight at 60°C in a vacuum oven. The results from the ICP analysis are summarized in Table 7. It is clear that increasing the temperature from 20°C to 60°C or 80°C results in a 50% or more reduction in the residual metal levels. Increasing the temperature from 60°C to 80°C helps further reduce the content of metals such as Fe, Mg and Mn.
[0092] Table 7: Inorganic content in samples from Example 4. "Metal" refers to the total metal content.
[0093]
[0094] Example 5 - Immersion Time
[0095] Kraft lignin powder (150 g) from the LignoBoost process was added to heated water (1.5 l, 60 ° C or 80 ° C) during stirring. After that, 7.5 g (5% by weight, based on the dry weight of the lignin added to the water) of oxalic acid or formic acid was added and the mixture was stirred at a maintained temperature for a period of time from 15 minutes to 4 hours. The mixture was then filtered and the lignin was collected and dried overnight in a vacuum oven at 60 ° C. For one sample (5d), the lignin was collected after filtration and subjected to a second immersion. All parameters were the same for both immersion steps, and the total immersion time was thus 8 hours. The experimental details are summarized in Table 8 and the results from the ICP analysis are summarized in Table 9. It can be seen that washing for 1 hour is sufficient to achieve a low total metal content of 86 ppm. However, it is also clear that the combination of higher temperatures and longer washing times produces the highest purity lignin. Two repeated washing tests at 80 ° C for 4 hours can bring all individual metal levels below 10 ppm except magnesium and a total metal level to 58 ppm.
[0096] Table 8: Experimental details for Example 5
[0097]
[0098] Table 9: Inorganic content in samples from Example 5. "Metal" refers to the total metal content.
[0099]
[0100] In view of the above detailed description of the present invention, other modifications and variations will become apparent to those skilled in the art. However, it should be apparent that such other modifications and variations can be implemented without departing from the spirit and scope of the present invention.
Claims
1. A method for purifying lignin, wherein the method comprises the following steps: a) providing lignin in solid form; b) providing an acidic aqueous solution having a pH below 6; c) immersing the lignin in the acidic aqueous solution for at least 15 minutes, wherein the temperature of the acidic aqueous solution during immersion is in the range of from 40° C. to 100° C., to remove metals from the lignin to the acidic aqueous solution, so as to obtain the purified lignin; d) separating the obtained purified lignin from the acidic aqueous solution; and e) optionally washing the separated purified lignin; Therein the lignin remains in solid form during all steps of the process.
2. The method according to claim 1, wherein the lignin provided in step a) is kraft lignin.
3. The method according to any one of claims 1 to 2, wherein the lignin provided in step a) has a total metal content of at least 500 ppm.
4. The method according to any one of claims 1 to 3, wherein the lignin provided in step a) has an aluminum content of at least 18 ppm; a calcium content of at least 18 ppm; an iron content of at least 16 ppm; a potassium content of at least 30 ppm; a magnesium content of at least 45 ppm; a manganese content of at least 11 ppm; and a sodium content of at least 400 ppm.
5. The method according to any one of claims 1 to 4, wherein the lignin is provided in the form of particles and wherein the particle size distribution of the lignin particles is such that at least 80% by weight of the particles have a diameter of less than 0.2 mm.
6. The method according to any one of claims 1 to 5, wherein the total amount of acid in the acidic aqueous solution is in the range from 0.1 to 6 wt. %, based on the dry weight of lignin immersed in the acidic aqueous solution.
7. The method according to any one of claims 1 to 6, wherein the acidic aqueous solution comprises at least one organic acid.
8. The method of claim 7, wherein the at least one organic acid is selected from the group consisting of formic acid and oxalic acid.
9. The method according to any one of claims 1 to 8, wherein the separation in step d) is performed using filtration.
10. The method according to any one of claims 1 to 9, wherein steps cd) and optionally e) are repeated at least once.
11. The process according to any one of claims 1 to 10, wherein the separated lignin is subjected to washing with an aqueous washing solution.
12. The process according to any one of claims 1 to 11, wherein the process comprises an additional step of drying the separated and optionally washed lignin.
13. The method according to any one of claims 1 to 12, wherein the purified lignin obtained has a total metal content of less than 200 ppm.
14. The method according to any one of claims 1 to 13, wherein the purified lignin obtained has an iron content of less than 15 ppm.
15. The method according to any one of claims 1 to 14, wherein the purified lignin obtained has a manganese content of less than 10 ppm.
16. The method according to any one of claims 1 to 15, wherein the purified lignin obtained has an aluminum content of less than 17 ppm; a calcium content of less than 16 ppm; a potassium content of less than 10 ppm; a magnesium content of less than 42 ppm; and a sodium content of less than 30 ppm.
17. Lignin having a total metal content of less than 200 ppm.
18. The lignin according to claim 17, wherein the lignin has an iron content of less than 15 ppm.
19. Lignin according to any one of claims 17-18, wherein the lignin has a manganese content of less than 10 ppm.
20. The lignin according to any one of claims 17-19, wherein the lignin has an aluminum content of less than 17 ppm; a calcium content of less than 16 ppm; a potassium content of less than 10 ppm; a magnesium content of less than 42 ppm; and a sodium content of less than 30 ppm.
21. The lignin according to any one of claims 17 to 20, wherein the lignin is kraft lignin.