Aqueous solution, coating agent, adhesive, paper processing agent, dispersant for emulsion polymerization, aqueous emulsion, laminate, and method for producing aqueous emulsion
By using a vinyl alcohol-based polymer aqueous solution containing carbonyl, formyl and alkenyl groups and a dispersant for emulsion polymerization, the insufficient performance of PVA in coating agents and aqueous emulsions is solved, and the coated paper and adhesive are realized. Excellent performance and improved mechanical stability and oil resistance of aqueous emulsions.
Patent Information
- Application Number
- CN202380031467.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, when PVA is an aqueous solution, a coating agent, an adhesive and a paper processing agent, there are problems such as insufficient storage stability, coating properties, breathability resistance, silicone curability and water resistance, and water resistance. The mechanical stability and oil resistance of the emulsion are poor.
Using an aqueous vinyl alcohol-based polymer solution containing carbonyl, formyl and alkenyl groups, an aqueous solution and an emulsion polymerization dispersant with excellent properties are produced through specific polymerization and saponification processes, and used to prepare coated paper and adhesives to improve the Its mechanical stability and oil resistance.
It realizes excellent storage stability, coating properties, breathable resistance, silicone curing properties and water resistance of coated paper, and the produced aqueous emulsion has significantly improved mechanical stability and oil resistance, which is suitable for various bonding and coating agent.
Smart Images

Figure BDA0005064641280000041 
Figure BDA0005064641280000042 
Figure BDA0005064641280000051
Abstract
Description
Technical Field
[0001] The present invention relates to an aqueous solution, a coating agent, an adhesive, a paper processing agent, a dispersant for emulsion polymerization, an aqueous emulsion, a laminate, and a method for producing the aqueous emulsion. Background Art
[0002] Vinyl alcohol polymer (hereinafter also referred to as "PVA") is known as a water-soluble synthetic polymer. In addition to its use as a fiber and film raw material, it is also widely used as a paper processing agent, a fiber processing agent, an inorganic binder, an adhesive, a stabilizer for emulsion polymerization and suspension polymerization, etc. In particular, a coating agent containing PVA as a main component is used as a paper processing agent. By applying PVA, which has excellent film-forming properties, to paper, it is possible to impart barrier properties and oil resistance to gases, etc.
[0003] Paper coated with PVA is sometimes used as barrier paper. As a representative example of barrier paper, release paper base paper can be cited. Release paper base paper is usually manufactured by coating PVA on the surface of a cellulose substrate. And, release paper is obtained by forming a release layer (silicone layer) on the surface of the release paper base paper. The PVA in the release paper plays the role of a filler that inhibits the penetration of expensive silicone and platinum into the substrate. Recently, a release paper base paper that can promote the curing of silicone in the release layer or improve the adhesion between the PVA layer and the silicone layer on the basis of this filling property is sought.
[0004] Patent Document 1 describes a cellulose substrate coated with PVA having double bonds introduced into the side chains by acetalization reaction. Generally, the acetalization reaction is carried out in water under acidic conditions, and a basic compound is added to perform a neutralization treatment. When the reaction solution is used as a coating agent, the solution stability of the coating agent is low due to a large amount of salt generated by the neutralization treatment.
[0005] Patent Document 2 describes a release paper obtained by coating a substrate with a coating agent containing PVA, wherein a double bond is introduced into the side chain by an esterification reaction. However, pyridine used in the esterification reaction may remain in the PVA and act as a catalyst poison to inhibit the curing reaction of the silicone in the release layer.
[0006] Patent document 3 describes a release paper obtained by applying a coating agent containing PVA having a double bond in a side chain to a substrate, wherein the PVA having a double bond in a side chain is obtained by esterifying PVA with a carboxylic acid having an unsaturated double bond or a salt thereof. Furthermore, if the coating agent is applied to the release paper, the packing property of the silicone in the release paper is excellent, and the curing of the silicone in the release layer can be promoted, and the adhesion between the substrate and the release layer can be improved. However, the PVA having a double bond in a side chain described in Patent document 3 also contains a component that is insoluble in water, and therefore, when used as a coating liquid, the coating property is insufficient.
[0007] Furthermore, adhesives with PVA as the main component are cheap and have excellent adhesion, and are used for bonding cardboard, corrugated cardboard, paper tubes, partitions, wallpaper, wood, etc. In addition, adhesives mixed with various emulsions and PVA are used as adhesives for woodworking purposes, fiber processing purposes, paper purposes, etc. Adhesives containing PVA in this way (PVA-based water-based adhesives) are used for a wide range of purposes. However, in PVA-based water-based adhesives, in order to cope with high-speed coating in recent years, for the purpose of improving adhesion, especially initial adhesion, various modified PVAs have been proposed.
[0008] As such modified PVA, alkyl-modified PVA is described in Patent Document 4. The PVA-based water-based adhesive obtained using such modified PVA has excellent initial adhesion, water-resistant adhesion, and storage stability of the adhesive. However, the water-resistant adhesion of the adhesive obtained using such modified PVA is insufficient.
[0009] Patent Document 5 describes an aldehyde-modified PVA. Furthermore, the adhesive containing the modified PVA is excellent in initial bonding strength, normal bonding strength, durable bonding strength, and shelf stability of the main agent. However, in the adhesive obtained using the modified PVA, there is room for improvement in initial bonding strength, and the effect when no curing agent is used is not disclosed.
[0010] In addition, PVA is also known as a protective colloid for emulsion polymerization of vinyl ester monomers represented by vinyl acetate. The aqueous emulsion obtained by emulsion polymerization using PVA as a dispersant for emulsion polymerization is widely used in the fields of various adhesives, coating bases, various binders for impregnated paper and nonwoven products, various coating agents, etc.
[0011] The aqueous emulsion synthesized by using PVA as a dispersant for emulsion polymerization has good adaptability in coating applications because (a) low molecular weight components do not migrate and adhesion to the substrate is excellent, and (b) viscosity is easy to adjust and coating properties are good. On the other hand, the monomers that can be generally used in such aqueous emulsions are limited to vinyl acetate and vinyl chloride with high free radical reactivity. Compared with the existing aqueous emulsions that use only surfactants as dispersion stabilizers, physical properties such as water resistance, oil resistance, mechanical stability, and freeze-thaw stability are insufficient, and improvement in this regard is expected.
[0012] In view of this, a technique for improving dispersibility by introducing a sulfonic group into PVA as a dispersant is described in Patent Document 6. However, in the emulsion produced by this method, PVA is often physically adsorbed to the polymer in the emulsion, and physical properties such as polymerization stability and mechanical stability are sometimes insufficient.
[0013] Patent Document 7 describes an aqueous emulsion using PVA containing diacetone acrylamide units as a dispersant and a polymer of ethylenically unsaturated monomers such as acrylic monomers, styrene monomers, and diene monomers as a dispersant. This PVA has excellent polymerization stability and mechanical stability, but in order to exhibit required physical properties such as water resistance and oil resistance, a crosslinking agent needs to be added separately.
[0014] In addition, a method for promoting the grafting reaction between PVA and dispersoids to obtain an aqueous emulsion having target properties has been proposed. Patent Document 8 describes the use of a polyvinyl alcohol-based polymer having a thiol group at the molecular end as a dispersant for emulsion polymerization. However, this PVA is synthesized by chain transfer polymerization, and a mixture of PVA having a thiol group and PVA without a thiol group is essentially obtained, so there are limitations in molecular design such as polymerization degree and thiol group introduction rate.
[0015] Prior art literature
[0016] Patent Literature
[0017] Patent Document 1: Japanese Patent Application No. 2013-531136
[0018] Patent Document 2: International Publication No. 2009 / 147283
[0019] Patent Document 3: International Publication No. 2018 / 124241
[0020] Patent Document 4: International Publication No. 2011 / 155546
[0021] Patent Document 5: Japanese Patent Application Publication No. 2006-52245
[0022] Patent Document 6: Japanese Patent Application Laid-Open No. 50-155579
[0023] Patent Document 7: Japanese Patent Application Publication No. 2001-220409
[0024] Patent Document 8: Japanese Patent Application Publication No. 2003-171567 Summary of the invention
[0025] Problems to be solved by the invention
[0026] The first object of the present invention is to provide an aqueous solution containing a vinyl alcohol polymer itself or a coated paper or the like produced using the aqueous solution, which is excellent in storage stability, coating properties, air resistance, silicone curing properties, adhesion between a release layer and a substrate, initial adhesion and water-resistant adhesion, as well as a coating agent, an adhesive and a paper processing agent containing the aqueous solution.
[0027] In addition, a second object of the present invention is to provide a dispersant for emulsion polymerization that can synthesize an aqueous emulsion, an aqueous emulsion containing such a dispersant for emulsion polymerization, a method for producing the same, and a laminate, wherein the aqueous emulsion is an aqueous emulsion that has excellent mechanical stability and generates little aggregates, and can produce coated paper, etc., that has excellent oil resistance.
[0028] Means used to solve problems
[0029] The aforementioned object is achieved by providing the following solution.
[0030] [1] An aqueous solution comprising a vinyl alcohol polymer having a carbonyl group, a formyl group and an alkenyl group in the same or different molecules;
[0031] [2] The aqueous solution according to [1], wherein the vinyl alcohol polymer has a structure represented by the following formula (1) containing the carbonyl group;
[0032] [Chemistry 1]
[0033]
[0034] In formula (1), m is an integer of 1 to 11.
[0035] [3] An aqueous solution comprising a vinyl alcohol polymer having a group represented by the following formula (2) at the end of the polymer chain;
[0036] [Chemistry 2]
[0037]
[0038] In formula (2), R 1 It is an alkenyl group.
[0039] [4] The aqueous solution according to [3], wherein R in the above formula (2) 1 The alkenyl group shown has a methylene group at the terminal end on the carbonyl side;
[0040] [5] The aqueous solution according to any one of [1] to [4], wherein the vinyl alcohol polymer has a tertiary carbon atom;
[0041] [6] The aqueous solution according to any one of [1] to [5], wherein the vinyl alcohol polymer has a structural unit derived from an aliphatic unsaturated aldehyde;
[0042] [7] The aqueous solution according to [6], wherein the aliphatic unsaturated aldehyde has 3 to 14 carbon atoms;
[0043] [8] The aqueous solution according to [6] or [7], wherein the aliphatic unsaturated aldehyde has a carbon-carbon double bond at the terminal end;
[0044] [9] The aqueous solution according to any one of [1] to [8], wherein the concentration of the vinyl alcohol polymer is 0.5% by mass or more and 30% by mass or less;
[0045]
[10] A coating agent comprising the aqueous solution of any one of [1] to [9];
[0046]
[11] An adhesive comprising the aqueous solution of any one of [1] to [9];
[0047]
[12] A paper processing agent comprising the aqueous solution of any one of [1] to [9];
[0048]
[13] A dispersant for emulsion polymerization, comprising a vinyl alcohol polymer having a carbonyl group, a formyl group and an alkenyl group in the same or different molecules;
[0049]
[14] The dispersant for emulsion polymerization according to
[13] , wherein the vinyl alcohol polymer has a structure represented by the following formula (1) containing the carbonyl group;
[0050] [Chemistry 3]
[0051]
[0052] In formula (1), m is an integer of 1 to 11.
[0053]
[15] A dispersant for emulsion polymerization, comprising a vinyl alcohol polymer having a group represented by the following formula (2) at the end of the polymer chain;
[0054] [Chemistry 4]
[0055]
[0056] In formula (2), R 1 It is an alkenyl group.
[0057]
[16] The dispersant for emulsion polymerization according to
[15] , wherein R in the above formula (2) 1 The alkenyl group shown has a methylene group at the terminal end on the carbonyl side;
[0058]
[17] The dispersant for emulsion polymerization according to any one of
[13] to
[16] , wherein the vinyl alcohol polymer has a tertiary carbon atom;
[0059]
[18] The dispersant for emulsion polymerization according to any one of
[13] to
[17] , wherein the vinyl alcohol polymer has a structural unit derived from an aliphatic unsaturated aldehyde;
[0060]
[19] The dispersant for emulsion polymerization according to
[18] , wherein the aliphatic unsaturated aldehyde has 3 to 14 carbon atoms;
[0061]
[20] The dispersant for emulsion polymerization according to
[18] or
[19] , wherein the aliphatic unsaturated aldehyde has a carbon-carbon double bond at the terminal;
[0062]
[21] The dispersant for emulsion polymerization according to any one of
[13] to
[20] , wherein the degree of saponification of the vinyl alcohol polymer is 80 mol% or more;
[0063]
[22] An aqueous emulsion comprising a polymer and the dispersant for emulsion polymerization according to any one of
[13] to
[21] , wherein the polymer comprises a structural unit derived from at least one selected from an ethylenically unsaturated monomer and a diene monomer;
[0064]
[23] The aqueous emulsion according to
[22] , wherein the ethylenically unsaturated monomer is at least one selected from styrene monomers, acrylate monomers and methacrylate monomers;
[0065]
[24] A laminate comprising a substrate and a layer formed from the aqueous emulsion of
[22] or
[23] ;
[0066]
[25] The laminate according to
[24] , wherein the substrate is paper.
[0067]
[26] A laminate comprising a substrate and a layer containing the dispersant for emulsion polymerization according to any one of
[13] to
[21] .
[0068]
[27] A method for producing an aqueous emulsion, comprising: emulsion polymerizing at least one monomer selected from an ethylenically unsaturated monomer and a diene monomer in the presence of the dispersant for emulsion polymerization described in any one of
[13] to
[21] ;
[0069]
[28] The method for producing an aqueous emulsion according to
[27] , wherein the ethylenically unsaturated monomer is at least one monomer selected from styrene-based monomers, acrylate-based monomers, and methacrylate-based monomers.
[0070] Effects of the Invention
[0071] The aqueous solution of the present invention or the coated paper etc. manufactured using the aqueous solution are excellent in storage stability, coating property, air permeability resistance, silicone curing property, adhesion between the peeling layer and the substrate, initial adhesion and water-resistant adhesion. Therefore, the aqueous solution can be suitably used in coating agents, adhesives, paper processing agents etc.
[0072] The dispersant for emulsion polymerization of the present invention can synthesize an aqueous emulsion having excellent mechanical stability and little generation of aggregates, and can produce coated paper having excellent oil resistance, etc. Therefore, the obtained aqueous emulsion can be suitably used in various adhesives, coatings, various binders, mixed materials, coating agents, laminates, etc. DETAILED DESCRIPTION
[0073] In the present specification, a numerical range described using "to" means that the numerical values described before and after "to" are included as the lower limit and the upper limit.
[0074] <Aqueous solution according to the first embodiment>
[0075] The aqueous solution according to the first aspect of the present invention contains a vinyl alcohol polymer (PVA) having a carbonyl group, a formyl group, and an alkenyl group in the same or different molecules, and water. The aqueous solution itself or a coated paper or the like produced using the aqueous solution has excellent storage stability, coating properties, air resistance, silicone curing properties, adhesion between a release layer and a substrate, initial adhesion, and water-resistant adhesion.
[0076] The aqueous solution may contain solvents other than water, such as organic solvents. The ratio of water in the solvent in the aqueous solution is preferably 50% by mass or more relative to the total amount of the solvent, more preferably 80% by mass or more, further preferably 90% by mass or more, and further preferably 95% by mass or more. In addition, the ratio of water in the solvent in the aqueous solution may be 100% by mass or less, or 99% by mass or less. In addition, the solvent in the aqueous solution is preferably substantially composed of water only.
[0077] The lower limit of the concentration of the PVA contained in the aqueous solution is not particularly limited, and for example, it is sometimes preferably 0.5 mass%, more preferably 1 mass%, further preferably 2 mass%, and further preferably 4 mass%. In addition, the upper limit of the concentration of the PVA contained in the aqueous solution is not particularly limited, and for example, it is sometimes preferably 30 mass%, more preferably 25 mass%, and further preferably 20 mass%. By making the concentration of the PVA in the aqueous solution within the above range, the coating efficiency is improved, and the high-speed coating property is more excellent.
[0078] The upper limit of the insoluble components in the aqueous solution is sometimes preferably 1000ppm, more preferably 500ppm, further preferably 200ppm, further preferably 100ppm, particularly preferably 70ppm, more particularly preferably 50ppm, and further particularly preferably 10ppm. In addition, the lower limit of the insoluble components in the aqueous solution is preferably 0ppm, and can be 1ppm. The insoluble components can be insoluble components in PVA. It should be noted that the insoluble components in the aqueous solution refer to: the mass ratio of the components dissolved and remaining in the aqueous solution to the total amount of PVA contained in the aqueous solution, specifically, it is measured using the following method.
[0079] The aqueous solution was passed through a metal filter with a mesh size of 63 μm, and the filter was further washed with warm water at 90° C. to obtain the solids remaining in the aqueous solution that were not dissolved. The ratio of the mass of the undissolved solids to the mass of the PVA contained in the aqueous solution before filtration was calculated and taken as the insoluble component in the aqueous solution.
[0080] The aqueous solution may contain other solutes except the PVA. As other solutes, water-soluble resins, surfactants, salts, etc. except the PVA may be listed. Wherein, the lower limit of the content of the PVA contained in the aqueous solution relative to all solutes is sometimes preferably 70% by mass, more preferably 80% by mass, further preferably 90% by mass, and further preferably 95% by mass, 99% by mass, or 99.9% by mass. The upper limit of the content of the PVA contained in the aqueous solution relative to all solutes may be 100% by mass, or 99.9% by mass, 99% by mass, or 95% by mass.
[0081] The aqueous solution is suitable for coating agents, adhesives, paper processing agents, etc. The method for producing the aqueous solution is not particularly limited. For example, it can be obtained by dissolving solid PVA in a solvent such as water.
[0082] <Vinyl alcohol polymer>
[0083] As described above, the PVA contained in the aqueous solution described in the first form of the present invention has a carbonyl group, a formyl group and an alkenyl group in the same or different molecules. The same is true for the PVA contained in the dispersant for emulsion polymerization described in the first form of the present invention described later. Below, the case where the PVA is used as a dispersant for emulsion polymerization is also explained. In the PVA, not all of the carbonyl groups, formyl groups and alkenyl groups may be contained in one molecule. That is, the PVA may be, for example, a mixture of PVA (a) having two groups among carbonyl groups, formyl groups and alkenyl groups and PVA (b) having the remaining one group. At this time, both PVA (a) and PVA (b) may have more than one group among carbonyl groups, formyl groups and alkenyl groups. The PVA may be a mixture of more than three types of PVA. It should be noted that the form of PVA having all of carbonyl, formyl and alkenyl groups in one molecule and the form of a mixture composed of multiple PVAs and having carbonyl, formyl and alkenyl groups have essentially the same properties. In addition, it is generally extremely difficult to distinguish these two forms by analysis, etc.
[0084] The PVA is a polymer having a vinyl alcohol unit as a structural unit. Generally, as described in detail later, the PVA can be obtained by polymerizing vinyl ester in the presence of an aliphatic unsaturated aldehyde, and the obtained vinyl ester polymer is saponified. The lower limit of the saponification degree of the PVA is not particularly limited, and for example, can be 20 mol%, 30 mol% or 40 mol%. The lower limit of the saponification degree of the PVA is sometimes preferably 65 mol%, more preferably 70 mol%, further preferably 75 mol%, and further preferably 80 mol%. And then, the lower limit of the saponification degree of the PVA is sometimes further preferably 82 mol%, 90 mol% or 92 mol%. By making the saponification degree of PVA be above the aforementioned lower limit, the solubility of the PVA in water is improved, the uniformity of the film surface coated with the aqueous solution is improved, the packing property of silicone is improved, and the bonding strength is further improved. On the other hand, the upper limit of the saponification degree of the PVA is not particularly limited, and can be 100 mol%, for example, sometimes preferably 99.99 mol%, more preferably 99.5 mol%, and further preferably 99 mol%. And then, the upper limit of the aforementioned saponification degree is sometimes further preferably 98 mol% or 96 mol%. By making the saponification degree of the PVA below the aforementioned upper limit, PVA is easily manufactured. In addition, by making the saponification degree of the PVA be the aforementioned range, when the PVA is used for emulsion polymerization dispersant, surface activity performance is suitable, etc., thus, each performance of the obtained aqueous emulsion (few coarse particles, excellent storage stability, suitable water resistance, etc.) is improved. The saponification degree is a value measured by the method described in JIS K6726:1994.
[0085] The carbonyl group (-C(=O)-) possessed by the PVA is a divalent group in which two connecting bonds are bonded to a carbon atom. That is, -C(=O)- in the formyl group (-C(=O)H) is not included in the carbonyl group possessed by the PVA. The PVA preferably has a structure represented by the following formula (1) containing a carbonyl group.
[0086] [Chemistry 5]
[0087]
[0088] In formula (1), m is an integer of 1 to 11. m is preferably an integer of 2 to 9 in some cases, and is preferably an integer of 3 to 7.
[0089] The content of the carbonyl group in the PVA is not particularly limited relative to the total content of the vinyl alcohol unit and the vinyl ester unit. As the lower limit, for example, it is sometimes preferably 0.001 mol%, more preferably 0.005 mol%, further preferably 0.008 mol%, and further preferably 0.01 mol%, 0.03 mol% or 0.05 mol%. As the upper limit of the content of the carbonyl group in the PVA, for example, it is sometimes preferably 5 mol%, more preferably 3 mol%, further preferably 1 mol%, and further preferably 0.3 mol% or 0.1 mol%. When the PVA is used as a dispersant for emulsion polymerization, the upper limit of the content of the carbonyl group in the PVA can be 0.05 mol%. When the content of the carbonyl group in the PVA is the aforementioned range, the various properties when the aqueous solution is used as, for example, a coating agent, an adhesive, etc. are improved. In addition, when the content of the carbonyl group in the PVA is the aforementioned range, the various properties when the PVA is used as a dispersant for emulsion polymerization are also improved. The content of the aforementioned carbonyl group is set to the value obtained by the method described in the embodiments described later.
[0090] The formyl group contained in the PVA is a monovalent group represented by -C(=O)H.
[0091] The content of the formyl group in the PVA is not particularly limited relative to the total content of the vinyl alcohol unit and the vinyl ester unit. As the lower limit, for example, it is sometimes preferably 0.01 mol%, more preferably 0.03 mol%, further preferably 0.05 mol%, and further preferably 0.07 mol% or 0.1 mol%. As the upper limit of the content of the formyl group in the PVA, for example, it is sometimes preferably 5 mol%, more preferably 3 mol%, further preferably 2 mol%, and further preferably 1 mol%, 0.8 mol% or 0.5 mol%. When the content of the formyl group in the PVA is the aforementioned range, the various properties when the aqueous solution is used as, for example, a coating agent, an adhesive, etc. are improved. In addition, when the content of the formyl group in the PVA is the aforementioned range, the various properties when the PVA is used as a dispersant for emulsion polymerization are also improved. The content of the aforementioned formyl group is set to the value obtained by the method described in the embodiments described later.
[0092] The alkenyl group of the PVA is a monovalent group formed by removing any one hydrogen atom from an olefin. The number of carbon atoms of the alkenyl group is sometimes preferably 2 to 13, more preferably 3 to 12, further preferably 4 to 11, and further preferably 5 to 9. The alkenyl group may be straight-chain or branched, preferably straight-chain. The alkenyl group is preferably located at the end of the polymer chain.
[0093] The alkenyl group of the PVA preferably has a carbon-carbon double bond at the terminal (front end). That is, the PVA preferably has a vinyl group at the terminal (front end). The alkenyl group of the PVA is more preferably a group represented by the following formula (5).
[0094] [Chemistry 6]
[0095]
[0096] In formula (5), n is an integer of 1 to 11. n is preferably an integer of 2 to 9, and more preferably an integer of 3 to 7.
[0097] The content of alkenyl in the PVA is not particularly limited relative to the total content of vinyl alcohol unit and vinyl ester unit, and as the lower limit, for example, it is sometimes preferably 0.005 mol%, more preferably 0.01 mol%, further preferably 0.02 mol%, further preferably 0.003 mol% or 0.04 mol%. As the upper limit of the content of alkenyl in the PVA, for example, it is sometimes preferably 5 mol%, more preferably 3 mol%, further preferably 1 mol%, further preferably 0.5 mol%, 0.3 mol% or 0.2 mol%. When the content of alkenyl in the PVA is the aforementioned range, the various properties when the aqueous solution is used as, for example, a coating agent, an adhesive, etc. are improved. In addition, when the content of alkenyl in the PVA is the aforementioned range, the various properties when the PVA is used as a dispersant for emulsion polymerization are also improved. The content of the aforementioned alkenyl is set to the value obtained by the method described in the embodiments described later. The suitable content range of vinyl in the PVA relative to the total content of vinyl alcohol unit and vinyl ester unit is the same as the suitable content range of the aforementioned alkenyl.
[0098] The PVA preferably has a terminal group derived from an aliphatic unsaturated aldehyde or a structural unit derived from an aliphatic unsaturated aldehyde. The aliphatic unsaturated aldehyde may have 3 to 14 carbon atoms, more preferably 4 to 12 carbon atoms, and even more preferably 6 to 10 carbon atoms.
[0099] The aforementioned aliphatic unsaturated aldehyde preferably has a carbon-carbon double bond, and more preferably has a carbon-carbon double bond at the end (front end). That is, the aforementioned aliphatic unsaturated aldehyde preferably contains a vinyl group. As the aforementioned aliphatic unsaturated aldehyde having a carbon-carbon double bond, it is preferably an aliphatic unsaturated aldehyde having an alkenyl group having a methylene group at the end of the carbonyl side, that is, an aliphatic unsaturated aldehyde having a group represented by R-CH2- (R is an alkenyl group). In other words, the aforementioned aliphatic unsaturated aldehyde is preferably an aliphatic unsaturated aldehyde other than α, β-unsaturated aldehyde. By using an aliphatic unsaturated aldehyde having a structure as described above, the reactivity during polymerization is improved, and PVA with a sufficient amount of functional groups (carbonyl groups, etc.) introduced can be effectively obtained.
[0100] The aliphatic unsaturated aldehyde is preferably a compound represented by the following formula (6).
[0101] [Chemistry 7]
[0102]
[0103] In formula (6), p is an integer of 1 to 11. p is preferably an integer of 2 to 9, and more preferably an integer of 3 to 7.
[0104] Examples of the aliphatic unsaturated aldehyde include 2-propenal, 3-butenal, 4-pentenal, 5-hexenal, 3-methyl-5-hexanal, 6-heptenal, 6-octenal, 7-octenal, 7-methyl-7-octenal, 3,7-dimethyl-7-octenal, 8-nonenal, 9-decenal, 10-undecenal, and 11-dodecenal.
[0105] Examples of the terminal group derived from an aliphatic unsaturated aldehyde preferably present in the PVA include a group represented by the following formula (2).
[0106] [Chemistry 8]
[0107]
[0108] In formula (2), R 1 It is an alkenyl group.
[0109] As R in formula (2) 1 The number of carbon atoms of the alkenyl group represented by R is preferably 2 to 13, more preferably 3 to 12, further preferably 4 to 11, and further preferably 5 to 9. 1 The alkenyl group shown may be straight-chain or branched, but is preferably straight-chain. 1 The alkenyl group represented by is sometimes preferably a group having a methylene group at the terminal of the carbonyl side (a group represented by R-CH2-(R is an alkenyl group)), more preferably a group having a carbon-carbon double bond at the terminal (front end), and further preferably a group represented by the above formula (5). The terminal group represented by formula (2) is usually formed when an aliphatic unsaturated aldehyde acts as a chain transfer agent.
[0110] Examples of the structural unit derived from an aliphatic unsaturated aldehyde preferably contained in the PVA include a structural unit represented by the following formula (3) or (4).
[0111] [Chemistry 9]
[0112]
[0113] In formulas (3) and (4), R 2 ~R 7 Each is independently a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. q is an integer of 1 to 11. r is an integer of 1 to 11.
[0114] R in formula (3) 2 ~R 4It is preferably a hydrogen atom. q is also preferably an integer of 2 to 9 in some cases, and more preferably an integer of 3 to 7. The structural unit represented by formula (3) is usually formed when an aliphatic unsaturated aldehyde acts as a monomer, and is introduced into the polymer chain.
[0115] R in formula (4) 5 ~R 7 It is preferably a hydrogen atom. r is also preferably an integer of 2 to 9, and more preferably an integer of 3 to 7. The structural unit represented by formula (4) is usually formed when the formyl group in the structural unit represented by formula (3) further functions as a chain transfer agent.
[0116] The PVA preferably has a tertiary carbon atom (a carbon atom directly bonded to three carbon atoms). In addition, the PVA preferably has a structural unit containing a tertiary carbon atom. In this case, that is, when the PVA has a branched structure, various properties when the aqueous solution is used as, for example, a coating agent, an adhesive, etc. are improved. In addition, when the PVA has a branched structure, various properties when the PVA is used as a dispersant for emulsion polymerization are also improved. The PVA, for example, has a structural unit represented by the above formula (3) or (4) and R 2 ~R 7 When it is a hydrogen atom, the PVA has a tertiary carbon atom.
[0117] The PVA may have other structural units in addition to the structural units derived from vinyl esters (vinyl alcohol units and vinyl ester units) and the structural units derived from aliphatic unsaturated aldehydes. Examples of monomers providing the aforementioned other structural units include α-olefins such as ethylene, propylene, 1-butene, isobutylene, and 1-hexene; acrylic acid, methacrylic acid; acrylic acid esters such as methyl acrylate and ethyl acrylate; methacrylic acid esters such as methyl methacrylate and ethyl methacrylate; acrylamide derivatives such as N-methylacrylamide, N-ethylacrylamide, and 2-acrylamide-2-methylpropanesulfonic acid; methacrylamide derivatives such as N-methylmethacrylamide and N-ethylmethacrylamide; maleic acid; maleic acid esters such as monomethyl maleate and dimethyl maleate; fumaric acid; fumaric acid esters such as monomethyl fumarate and dimethyl fumarate; itaconic acid; 3,4-diacetoxy-1-butene; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, and n-butyl vinyl ether; Ethylene glycol vinyl ether, 1,3-propylene glycol vinyl ether, 1,4-butanediol vinyl ether and other vinyl ethers containing hydroxyl groups; allyl acetate; allyl ethers such as propyl allyl ether, butyl allyl ether, hexyl allyl ether and other allyl ethers; monomers having oxyalkylene groups; isopropenyl acetate; hydroxyl-containing α-olefins such as 3-butene-1-ol, 4-pentene-1-ol, 5-hexene-1-ol, 7-octen-1-ol, 9-decen-1-ol, 3-methyl-3-butene-1-ol and other hydroxyl-containing α-olefins; vinyltrimethoxysilane, vinylmethyldimethoxysilane, vinyldimethylmethoxysilane, vinyltriethoxysilane, vinylmethyldiethoxysilane, vinyldimethylethoxysilane, 3-(meth)acrylamidepropyltrimethoxysilane, 3-(meth)acrylamidepropyltriethoxysilane and other monomers having silyl groups;
[0118] The ratio of the aforementioned other structural units in all the structural units in the PVA is sometimes preferably less than 20 mol%, sometimes more preferably less than 20 mol%, and sometimes more preferably less than 10 mol%, 5 mol% or 1 mol%. On the other hand, the ratio of the aforementioned other structural units can be, for example, more than 0.1 mol%, or more than 1 mol%. The ratio of the ethylene units in all the structural units in the PVA is sometimes also preferably less than 20 mol%, and sometimes more preferably less than 10 mol%, 5 mol% or 1 mol%. On the other hand, the ratio of the aforementioned ethylene units can be, for example, more than 0 mol%, or more than 1 mol%.
[0119] The lower limit of the viscosity average degree of polymerization of the PVA is not particularly limited, and may be, for example, 50 or 100, and may be preferably 200, more preferably 300, further preferably 400, and further preferably 500. By making the viscosity average degree of polymerization equal to or greater than the aforementioned lower limit, the protective colloid property is improved, and various properties when the PVA is used, for example, as a dispersant for emulsion polymerization are improved. From the viewpoint of the packing property of silicone when the aqueous solution is used as a coating agent, the viewpoint of the bonding strength when used as an adhesive, etc., the viscosity average degree of polymerization of the PVA is sometimes particularly preferably 1,000 or more. On the other hand, the upper limit of the viscosity average degree of polymerization is not particularly limited, and may be, for example, preferably 5,000, more preferably 3,000, and further preferably 2,000 or 1,500. In addition, when the PVA is used as a dispersant for suspension polymerization, etc., the upper limit of the viscosity average degree of polymerization may be 1,000. By making the viscosity average degree of polymerization equal to or less than the aforementioned upper limit, the surface active property is improved, and various properties when used, for example, as a dispersant for emulsion polymerization are improved. The viscosity average degree of polymerization is a value measured in accordance with JIS K6726: 1994. Specifically, it can be determined by the following formula from the intrinsic viscosity [η] (unit: liter / g) measured in water at 30°C after re-saponifying PVA to a saponification degree of 99.5 mol% or more and purifying it.
[0120] Viscosity average degree of polymerization = ([η] × 10 4 / 8.29) (1 / 0.62)
[0121] The water-insoluble components in the PVA are preferably less than 1000ppm. The upper limit of the water-insoluble components is sometimes preferably 500ppm, more preferably 200ppm, and further preferably 100ppm, 70ppm, 50ppm or 10ppm. In addition, the lower limit of the water-insoluble components of PVA can be 0ppm or 1ppm. Here, the water-insoluble components refer to the mass ratio of the components that are dissolved and remain after PVA is added to water in a concentration of 5% by mass and stirred at 90°C for 60 minutes. Specifically, it is measured by the following method.
[0122] That is, a 500mL flask equipped with a stirrer and a reflux condenser is prepared in a water bath set to 20°C, 285g of distilled water is added to the flask, and stirring is started at 300rpm. 15g of PVA is weighed and slowly added to the flask. After all the PVA (15g) is added, it takes 30 minutes to raise the temperature of the water bath to 90°C, thereby dissolving the PVA and obtaining a PVA solution. After the temperature of the water bath reaches 90°C, it is further stirred at 300rpm for 60 minutes while continuing to dissolve. Thereafter, the aforementioned PVA solution is used to filter the undissolved and residual PVA solids (hereinafter sometimes referred to as "insoluble solids" or "insoluble particles") using a metal filter with a mesh of 63μm. Next, the filter is washed with warm water at 90°C to remove the PVA solution attached to the filter. After only insoluble solids remain on the filter, the filter is dried in a heating dryer at 120°C for 1 hour. The mass of the filter after drying was compared with the mass of the filter before filtration to calculate the mass of the insoluble solids. The ratio of the mass of the insoluble solids to the mass (15 g) of PVA initially added to the water was defined as the water-insoluble component.
[0123] The substance separated in the form of PVA can contain trace components such as sodium atoms (Na). For example, sodium atoms can interact with PVA in the state of sodium ions, or can be mixed with PVA in the state of sodium salts. It should be noted that in this specification, the substance containing such trace components is sometimes referred to as PVA. The upper limit of the Na content in PVA is sometimes preferably 8% by mass, more preferably 5% by mass, further preferably 1% by mass, further preferably 0.6% by mass, and particularly preferably 0.3% by mass. The lower limit of the Na content in PVA is not particularly limited, and can be 0% by mass, or 0.01% by mass or 0.1% by mass. It should be noted that the sodium Na content in PVA is measured by the method described in the embodiments described below.
[0124] The aqueous solution may contain sodium atoms. The sodium atoms may exist in the form of sodium ions or sodium salts. The upper limit of the sodium atom (Na) content relative to the solid component in the aqueous solution is sometimes preferably 8% by mass, more preferably 5% by mass, further preferably 1% by mass, further preferably 0.6% by mass, and particularly preferably 0.3% by mass. The lower limit of the Na content relative to the aforementioned solid component is not particularly limited, and may be 0% by mass, or 0.01% by mass or 0.1% by mass.
[0125] <Aqueous solution according to the second embodiment>
[0126] The aqueous solution described in the second embodiment of the present invention contains PVA having a group represented by the following formula (2) at the end of the polymer chain and water. The aqueous solution itself or the coated paper produced using the aqueous solution is excellent in storage stability, coating properties, air permeability resistance, silicone curing properties, adhesion between the peeling layer and the substrate, initial adhesion and water-resistant adhesion. In the aqueous solution described in the second embodiment of the present invention, the suitable forms of PVA concentration, amount of insoluble components, other components, use, etc. are the same as the suitable forms of the aqueous solution described in the first embodiment of the present invention.
[0127] [Chemistry 10]
[0128]
[0129] In the aforementioned PVA, R in formula (2) 1 It is an alkenyl group. The specific form and suitable form of the group (terminal group) represented by the above formula (2) are as described above. As described above, the group represented by the above formula (2) is introduced to the end of the polymer chain when the aliphatic unsaturated aldehyde acts as a chain transfer agent when the vinyl ester is polymerized in the presence of an aliphatic unsaturated aldehyde. The PVA can be formed by only one type of PVA or a mixture of two or more types of PVA. The specific form and suitable form of the PVA contained in the aqueous solution described in the second form of the present invention are the same as the specific form and suitable form of the PVA contained in the aqueous solution described in the first form of the present invention, except that it is not necessary to "have a carbonyl group, a formyl group and an alkenyl group in the same or different molecules".
[0130] The PVA may have a carbon-carbon double bond in addition to the alkenyl group, and particularly preferably has -CO-(CH=CH) p - (p is an integer of 1 to 5). The above structure is introduced by, for example, heat-treating PVA.
[0131] <Method for producing vinyl alcohol polymer>
[0132] The PVA of the present application is produced through the following steps: a step of polymerizing a vinyl ester in the presence of an aliphatic unsaturated aldehyde (step A); and a step of saponifying the obtained vinyl ester polymer (step B).
[0133] (Process A)
[0134] In step A, vinyl ester is polymerized in the presence of an aliphatic unsaturated aldehyde to obtain a vinyl ester polymer. As methods for polymerizing vinyl ester, known methods such as bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization can be cited. Among these methods, bulk polymerization under solvent-free conditions and solution polymerization using solvents such as alcohols are preferred. As the aforementioned alcohol, an alcohol having a carbon number of 3 or less is preferred, more preferably methanol, ethanol, n-propanol, and isopropanol, and further preferably methanol. When the polymerization reaction is carried out by these methods, the reaction mode can be any of an intermittent mode and a continuous mode. There is no particular limitation on the polymerization temperature when the polymerization reaction is carried out, and it is suitable to be in the range of above 5°C and below 200°C.
[0135] Examples of the vinyl ester include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, and vinyl versatate. Among them, vinyl acetate is preferred.
[0136] Examples of the polymerization initiator used in the polymerization reaction include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile); and organic peroxide initiators such as benzoyl peroxide, n-propyl peroxycarbonate, and diisopropyl peroxydicarbonate. The amount of the polymerization initiator used is preferably 0.01 to 5% by mass relative to the vinyl ester used.
[0137] Specific examples and suitable examples of aliphatic unsaturated aldehydes present during the polymerization of vinyl esters are as described above. One or more aliphatic unsaturated aldehydes can be used. As the amount of aliphatic unsaturated aldehydes used, for example, it is preferably 0.1 to 10% by mass relative to vinyl ester. In the polymerization of vinyl esters, other chain transfer agents other than aliphatic unsaturated aldehydes may also coexist. As other chain transfer agents, aliphatic saturated aldehydes such as acetaldehyde, propionaldehyde, butyraldehyde, 1-pentanal, 1-hexanal, 1-octanal, 1-nonanal, 1-decanal, etc.; ketones such as acetone and methyl ethyl ketone; mercaptans such as 2-hydroxyethanethiol and 3-mercaptopropionic acid; thiocarboxylic acids such as thioacetic acid; halogenated hydrocarbons such as trichloroethylene and perchloroethylene, etc. can be listed.
[0138] When the vinyl ester is polymerized, a copolymerizable monomer may be further copolymerized within a range that does not impair the gist of the present invention. Examples of the copolymerizable monomer include the monomers described above as monomers providing other structural units.
[0139] (Process B)
[0140] In step B, the vinyl ester polymer obtained by step A is saponified in, for example, an alcohol solution using an alkali catalyst or an acid catalyst to obtain PVA. The saponification reaction of the vinyl ester polymer can be applied to an alcohol decomposition or hydrolysis reaction using an alkaline catalyst such as sodium hydroxide, potassium hydroxide, sodium methoxide, or an acidic catalyst such as p-toluenesulfonic acid. As the solvent used in the saponification reaction, alcohols such as methanol and ethanol; esters such as methyl acetate and ethyl acetate; ketones such as acetone and methyl ethyl ketone; aromatic hydrocarbons such as benzene and toluene, etc. can be listed. They can be used alone or in combination of two or more. Among these, it is simple to use methanol or a mixed solution of methanol and methyl acetate as a solvent and to carry out a saponification reaction in the presence of sodium hydroxide as an alkaline catalyst, so it is preferred. Saponification can be carried out using a belt reactor, a kneader reactor, a tower reactor, etc.
[0141] A resin solid material containing PVA is obtained by going through step B. In this production method, as steps after step B, there may be further steps of washing the resin solid material containing PVA, drying the resin solid material containing PVA, heat treating the resin solid material containing PVA, etc.
[0142] <Coating agent>
[0143] One embodiment of the present invention is a coating agent comprising the above-mentioned aqueous solution. The aqueous solution contained in the coating agent may be the aqueous solution described in the first embodiment, or the aqueous solution described in the second embodiment, or both. The use of the coating agent is not particularly limited, for example, it may be a coating agent for a paper substrate or a film substrate, or it may be a coating agent used in the manufacture of release paper or a release film.
[0144] The coating agent may contain an organic solvent, or may contain water-insoluble organic particles, inorganic particles, and the like.
[0145] The lower limit of the concentration of PVA contained in the coating agent is not particularly limited, for example, it is sometimes preferably 1 mass%, more preferably 2 mass%, and further preferably 4 mass%. In addition, the upper limit of the concentration of PVA contained in the coating agent is not particularly limited, for example, it is sometimes preferably 30 mass%, and more preferably 25 mass%. By making the concentration of PVA in the coating agent within the above range, the coating efficiency is further improved, and the high-speed coating property is more excellent.
[0146] The upper limit of the insoluble components in the coating agent is sometimes preferably 1,000 ppm, more preferably 500 ppm, further preferably 200 ppm, further preferably 100 ppm, particularly preferably 70 ppm, further particularly preferably 50 ppm, and further particularly preferably 10 ppm. In addition, the lower limit of the insoluble components in the coating agent is preferably 0 ppm, and may be 1 ppm. It should be noted that the insoluble components in the coating agent refer to the ratio of the mass of the components dissolved and remaining in the coating agent to the total amount of PVA contained in the coating agent, and are specifically measured by the following method.
[0147] The coating agent is passed through a metal filter with a mesh size of 63 μm, and the filter is further washed with warm water at 90°C to obtain solids that are not dissolved in the coating agent and remain. The ratio of the mass of the undissolved solids to the mass of the PVA contained in the coating agent before filtration is calculated and is set as the insoluble component in the coating agent.
[0148] The method for producing the coating agent is not particularly limited, and the coating agent can be obtained, for example, by dissolving PVA particles in a solvent such as water.
[0149] The coating agent may contain other components in addition to the aforementioned PVA and solvent within a range that does not impair the effects of the present invention. Other components include water-based dispersible resins such as SBR, NBR, polyvinyl acetate, ethylene vinyl acetate copolymer, poly(meth)acrylate, and polyvinyl chloride; raw starch obtained from wheat, corn, rice, potato, sweet potato, cassava, and sago palm; raw starch decomposition products such as oxidized starch and dextrin; starch derivatives such as etherified starch, esterified starch, and cationized starch; cellulose derivatives such as methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose (CMC); monosaccharides such as glucose, fructose, isomerized sugar, and xylose; maltose, Disaccharides such as lactose, sucrose, trehalose, palatinose, reduced maltose, reduced palatinose, and reduced lactose; oligosaccharides such as starch syrup, isomaltooligosaccharide, fructooligosaccharide, lactose oligosaccharide, soybean oligosaccharide, xylooligosaccharide, coupling sugar, and cyclodextrin compounds; polysaccharides such as pullulan, pectin, agar, konjac, polydextrose, and xanthan gum; albumin, gelatin, casein, gum arabic, polyamide resin, melamine resin, poly(meth)acrylamide, polyvinyl pyrrolidone, sodium poly(meth)acrylate, anion-modified PVA, sodium alginate, and water-soluble polyester. The content of these components (water-soluble resin and water-dispersible resin) in the coating agent is preferably 10% by mass or less.
[0150] The coating agent may contain a pigment within the scope of not damaging the effect of the present invention. As the pigment, inorganic pigments (clay, kaolin, aluminum hydroxide, calcium carbonate, talc, etc.) and organic pigments (plastic pigments, etc.) commonly used in the field of coated paper manufacturing may be cited. The content of these pigment components in the coating solution is preferably below 50% by mass.
[0151] The coating substrate of the coating agent of the present invention is not particularly limited, and examples thereof include paper, films, etc. Among them, the coating substrate of the coating agent of the present invention is preferably paper.
[0152] <Paper processing agent>
[0153] One embodiment of the present invention is a paper processing agent comprising the above-mentioned aqueous solution. The paper processing agent can be used by, for example, applying it to paper as a substrate. When the paper processing agent is applied to paper as a substrate for use, the paper processing agent in this form is an example of a coating agent. In addition, in the processing of paper, the paper processing agent can also be used as an adhesive for paper.
[0154] As the paper used in the substrate, known paper and synthetic paper obtained by papermaking chemical pulps such as hardwood kraft pulp and softwood kraft pulp, GP (wood pulp), RGP (refined machine pulp), TMP (thermomechanical pulp) and other mechanical pulps can be used. In addition, as paper, high-quality paper, medium-quality paper, alkaline paper, glass paper, semi-glass paper, etc. can also be used. In addition, cardboard and white cardboard used for corrugated board applications, building materials applications, white board applications, particle board applications, etc. can also be used. It should be noted that paper can contain papermaking auxiliary chemicals such as organic pigments or inorganic pigments, paper strength enhancers, sizing agents, and yield improvers. In addition, the paper can be subjected to various surface treatments.
[0155] In addition, a suitable embodiment of the present invention is a release paper base paper obtained by applying the above-mentioned paper processing agent to paper. When a release layer is formed on the release paper base paper, the above-mentioned coating agent plays the role of a packing agent. In other words, the release paper base paper obtained by applying the above-mentioned coating agent to paper is obtained by forming a packing layer on a substrate. The method for manufacturing the release paper base paper is not particularly limited, but preferably a method comprising a step of applying the coating agent to a substrate and a step of drying the substrate after the coating. The above-mentioned paper can be used.
[0156] The coating of the paper processing agent of the present invention can be carried out using general equipment for coated paper. For example, an on-machine coater or off-machine coater equipped with a coating device such as a knife coater, an air knife coater, a transfer roll coater, a bar metering size press coater, a curtain coater, a wire rod coater, etc. can be used to apply the coating liquid in one or more layers on the paper substrate. In addition, various heating and drying methods such as hot air heating, gas heater heating, infrared heater heating, etc. can be appropriately used as a drying method after coating. The coating amount is preferably 0.3 to 5.0 g / m in terms of dry mass. 2 By making the coating amount 0.3g / m 2 The coating amount is more preferably 0.5 g / m 2 On the other hand, by setting the coating amount to 5.0 g / m 2 The coating amount is preferably 3.0 g / m 2 the following.
[0157] As a method for judging the packing effect of the packing layer, the air permeability measured by using a Wangyan smoothness air permeability tester in accordance with JIS P8117:2009 can be used. The air permeability is sometimes preferably 1000 sec or more, more preferably 5000 sec or more, further preferably 10000 sec or more, and particularly preferably 50000 sec or more. When the air permeability is within the above range, the packing effect is better. It should be noted that the smaller the air permeability value (seconds; sec), the faster the air permeability.
[0158] In order to improve the packing effect, after applying the paper processing agent, the paper is dried and smoothed within the range that does not impair the effect. As the smoothing treatment, a super calender, a gloss calender, a multi-nip calender, a soft calender, a belt nip calender, etc. can be preferably used.
[0159] In addition, a release paper having the above-mentioned release paper base and a release layer formed on the surface of the release paper base is also a suitable embodiment of the present invention. In this case, the above-mentioned release layer preferably contains addition-type silicone and platinum, and preferably contains 0.001 mass parts or more and 0.05 mass parts or less of platinum relative to 100 mass parts of addition-type silicone. By making the blending amount of platinum within this range, a release paper with excellent curing properties can be obtained. The blending amount of platinum is sometimes preferably 0.002 mass parts or more, and more preferably 0.004 mass parts or more. In addition, the blending amount of platinum is sometimes preferably 0.03 mass parts or less, and more preferably 0.02 mass parts or less.
[0160] Addition silicone can be obtained by subjecting an organopolysiloxane having at least two SiH groups and a reactive carbon-carbon double bond in one molecule to a hydrosilylation reaction with an organohydrogenpolysiloxane having at least two SiH groups in one molecule in the presence of a platinum catalyst.
[0161] The organopolysiloxane containing at least 2 SiH groups and reactive carbon-carbon double bonds in one molecule is preferably an organopolysiloxane containing at least 2 vinyl groups, allyl groups, propenyl groups, isopropenyl groups, butenyl groups, isobutenyl groups, hexenyl groups and other carbon-carbon double bonds in one molecule. The organopolysiloxane can be exemplified by a material having a repeating unit of a diorganosiloxane as the main chain and a triorganosiloxane structure at the end, and can have a branched or cyclic structure. As an organic group bonded to silicon in the end or repeating unit, methyl, ethyl, phenyl, etc. can be exemplified. As a specific example, a methylphenyl polysiloxane having vinyl groups at both ends can be cited.
[0162] An organohydrogenpolysiloxane containing at least two SiH groups in one molecule is an organopolysiloxane containing two or more SiH groups at the terminal and / or in a repeating structure. Examples of such organopolysiloxanes include those having a diorganosiloxane repeating unit as the main chain and a triorganosiloxane structure at the terminal, and may have a branched or cyclic structure. Examples of organic groups bonded to silicon at the terminal and in the repeating unit include methyl, ethyl, octyl, phenyl, etc., and two or more of these groups may be replaced with hydrogen.
[0163] The addition type silicone is appropriately selected from solvent type, solvent-free type, and emulsion type. From the perspective of reducing environmental burden and coating properties, solvent-free type addition type silicone is preferably used. These silicones do not necessarily need to be used alone, and two or more types may be mixed and used as needed.
[0164] Generally, a platinum catalyst can be used for curing of silicone, and the type of platinum catalyst used in the present invention is not particularly limited. It is suitable to use a substance that cures addition silicone by hydrosilylation reaction. The platinum catalyst does not necessarily need to be used alone, and two or more types can be mixed and used as needed. The platinum in the platinum catalyst is quantified by using an ICP emission spectrometer, so as to determine the amount of platinum mixed.
[0165] The release layer in the release paper may also contain other components in addition to the addition type silicone and platinum within the range that does not impair the effect of the present invention. The amount of the other components is usually 30 parts by mass or less relative to 100 parts by mass of the total amount of the release layer. Examples of the other components include viscosity modifiers, adhesion improvers, defoamers, plasticizers, water resistance agents, preservatives, antioxidants, penetrants, surfactants, inorganic pigments, organic pigments, fillers, starch and its derivatives, cellulose and its derivatives, sugars, latex, etc.
[0166] The method for producing the release paper is not particularly limited, and the following method is used: after applying a coating agent on a substrate to form a plugging layer, the release layer is prepared in such a manner that the amount of platinum blended relative to 100 parts by mass of the addition-type silicone is 0.001 to 0.05 parts by mass, and the coating liquid containing a platinum catalyst obtained in this way is applied on the plugging layer to form the release layer. The coating amount of the coating liquid containing a platinum catalyst to form the release layer is not particularly limited, but is preferably 0.1 to 5 g / m in terms of solid content from the viewpoint of better release properties. 2 The coating amount is more preferably 0.3 g / m 2 When the coating amount is within the above range, the adhesion between the release layer containing addition silicone and platinum and the plugging layer is improved. The coating amount is more preferably 3 g / m 2 Various coating methods can be used, and knife coater, air knife coater, bar coater, etc. are suitable.
[0167] <Adhesive>
[0168] One embodiment of the present invention is an adhesive comprising the aqueous solution. The adhesive may contain other additives and the like.
[0169] The concentration range of PVA contained in the adhesive is not particularly limited, but is preferably 0.5 mass % to 30 mass %, more preferably 1 mass % to 20 mass %, from the viewpoints of coating properties, adhesion, strength of the bonded portion, water resistance, etc.
[0170] The adhesive according to one preferred embodiment of the present invention has excellent initial adhesion. The mechanism is not clear, but it is believed that the alkenyl groups of PVA in the adhesive function more effectively as hydrophobic groups, and form pseudo-associates in water through the interaction of the hydrophobic groups, which increases the viscosity and thus exhibits initial adhesion. However, the adhesive of the present invention is not limited to those exhibiting this mechanism.
[0171] The adhesive may contain an aqueous solution of the aforementioned PVA and a polymer or filler in an emulsion state. Furthermore, the adhesive may contain other additives. Other additives include dispersants such as metal salts of phosphoric acid compounds such as sodium polyphosphate and sodium hexametaphosphate, inorganic substances such as water glass, anionic polymer compounds such as polyacrylic acid and its salts, sodium alginate, and α-olefin-maleic anhydride copolymers, and their metal salts, nonionic surfactants such as polyethylene oxide, ethylene oxide adducts of higher alcohols, and copolymers of ethylene oxide and propylene oxide, cellulose derivatives such as carboxymethyl cellulose and methyl cellulose, and defoamers, preservatives, mildew inhibitors, coloring pigments, deodorants, fragrances, and the like.
[0172] The adhesive can improve the adhesiveness by containing the polymer in the emulsion state, and can reduce the burden during drying caused by the increase of the solid content. The polymer contained in the emulsion state (hereinafter also referred to as polymer emulsion) is not particularly limited, and is preferably a polymer (including copolymer) obtained from at least one monomer selected from ethylene unsaturated monomers and diene monomers.
[0173] Examples of the ethylenically unsaturated monomer include olefins such as ethylene, propylene, and isobutylene; vinyl esters such as vinyl acetate; (meth)acrylates such as methyl acrylate, ethyl acrylate, and butyl acrylate; and styrene.
[0174] In addition, examples of the diene monomer include butadiene, isoprene, and chloroprene.
[0175] Specific examples of such polymer emulsions include vinyl acetate emulsions such as vinyl acetate polymers, vinyl acetate-ethylene copolymers, vinyl acetate-versatate vinyl copolymers, and vinyl acetate-(meth)acrylate copolymers; (meth)acrylate emulsions such as methyl methacrylate / n-butyl acrylate copolymers; styrene emulsions; butadiene emulsions such as styrene-butadiene copolymers and methyl methacrylate-butadiene copolymers; and the like.
[0176] Among these, vinyl acetate emulsion particles or (meth)acrylate emulsion particles are preferred from the viewpoint of the initial adhesiveness and storage stability of the adhesive.
[0177] The polymer emulsion particles can improve the stability of the emulsion state by containing a dispersion stabilizer. As the dispersion stabilizer, vinyl alcohol polymers, water-soluble cellulose derivatives such as hydroxyethyl cellulose, various surfactants, etc. can be used, among which vinyl alcohol polymers are preferred.
[0178] The upper limit of the content of these emulsions (polymer emulsion particles and dispersion stabilizer) is not particularly limited, for example, based on the solid content, relative to 100 parts by mass of PVA, it is usually preferably 1,000 parts by mass or less, more preferably 700 parts by mass or less, and further preferably 500 parts by mass or less. On the other hand, the lower limit of the above content is not particularly limited, for example, it can be used at 100 parts by mass or more.
[0179] When the adhesive further contains a filler, the burden during drying can be reduced due to an increase in solid content, and the strength and hardness after bonding can be improved.
[0180] Examples of fillers include clays such as kaolinite, halloysite, pyrophyllite, or sericite; heavy, light, or surface-treated calcium carbonate; inorganic fillers such as aluminum hydroxide, aluminum oxide, gypsum, talc, and titanium oxide; and organic fillers such as starch, oxidized starch, wheat flour, and wood flour. Among these, various clays and various starches can be preferably used.
[0181] The upper limit of the content of the filler is not particularly limited, and for example, based on the solid content, it is sometimes preferably 1,000 parts by mass or less, more preferably 500 parts by mass or less, and further preferably 400 parts by mass or less and 50 parts by mass or more relative to 100 parts by mass of PVA. By making the content of the filler within the above range, there is a tendency to suppress the sedimentation of the filler during storage and improve the storage stability.
[0182] The preparation method of the adhesive is not particularly limited, and a known method can be used. For example, the following method can be listed: a substance pre-mixed with PVA and other additives such as fillers is added to water while stirring, or various additives, fillers, and PVA are added to water one by one while stirring, and a slurry is prepared, and then heated and dissolved. As a heating method at this time, a heating method of directly blowing steam into the slurry; a known heating method such as an indirect heating method based on a jacket can be used. The preparation can be carried out by either an intermittent method or a continuous method.
[0183] The adhesive described in a suitable embodiment of the present invention has excellent water solubility and initial adhesion, and also has excellent storage stability such as viscosity stability and sedimentation stability. In addition, by adjusting the aforementioned PVA contained, the water resistance after bonding can also be improved. Therefore, the aforementioned adhesive can be suitably used as a paper adhesive used during the manufacture or use of corrugated cardboard, paper bags, cartons, paper tubes, wallpapers, etc.; a woodworking adhesive for bonding wood to each other, wood to fiber, wood to paper, and wood to plastic. In addition, it can also be used for uses with fibers such as cloth and non-woven fabrics, cement molded objects such as concrete, various plastics, aluminum foil, etc. as bonded materials. It should be noted that the use of the adhesive of the present invention is not limited to them.
[0184] The viscosity of the adhesive can be arbitrarily selected according to the application. When high-speed coating properties are desired, the viscosity at the sticking temperature is preferably 100 to 10,000 mPa·s in terms of B-type viscosity.
[0185] <Dispersant for emulsion polymerization according to the first embodiment>
[0186] The dispersant for emulsion polymerization described in the first form of the present invention is a dispersant for emulsion polymerization of PVA having carbonyl, formyl and alkenyl groups in the same or different molecules. By using the dispersant for emulsion polymerization, an aqueous emulsion can be synthesized, which is an aqueous emulsion with excellent mechanical stability and less generation of aggregates, and can produce coated paper with excellent oil resistance. The dispersant for emulsion polymerization can be suitably used as an emulsion polymerization dispersant of at least one monomer selected from olefin monomers, vinyl ester monomers, (meth) acrylate monomers, acrylamide monomers, styrene monomers, diene monomers and halogen vinyl monomers. The dispersant for emulsion polymerization can also be used as a dispersant for emulsion polymerization of diene monomers. The PVA used in the dispersant for emulsion polymerization of this form and its specific form and suitable form are the same as the specific form and suitable form of the PVA contained in the aqueous solution described in the first form of the present invention. The method for manufacturing PVA is also as described above.
[0187] The dispersant for emulsion polymerization can be composed of only the PVA, or can also contain other components. As other components, existing known dispersants for emulsion polymerization can be listed. The lower limit of the content of the PVA in the dispersant for emulsion polymerization is sometimes preferably 70% by mass, more preferably 80% by mass, further preferably 90% by mass, and further preferably 95% by mass, 99% by mass or 99.9% by mass. The upper limit of the content of the PVA in the dispersant for emulsion polymerization can be 100% by mass, or 99.9% by mass, 99% by mass or 95% by mass.
[0188] <Dispersant for emulsion polymerization according to the second embodiment>
[0189] The dispersant for emulsion polymerization described in the second aspect of the present invention is a dispersant for emulsion polymerization containing PVA having a group represented by the following formula (2) at the end of the polymer chain. By using this dispersant for emulsion polymerization, an aqueous emulsion can be synthesized, and the aqueous emulsion is an aqueous emulsion that is excellent in mechanical stability and generates little aggregates, and coated paper with excellent oil resistance can be produced.
[0190] [Chemistry 11]
[0191]
[0192] In formula (2), R 1It is an alkenyl group. The specific form and suitable form of the group (terminal group) represented by the above formula (2) are as described above. As described above, the group represented by the above formula (2) is introduced into the end of the polymer chain when the aliphatic unsaturated aldehyde acts as a chain transfer agent when the vinyl ester is polymerized in the presence of an aliphatic unsaturated aldehyde. The PVA can be formed by only one type of PVA, or it can be a mixture of two or more types of PVA. The specific form and suitable form used in the dispersant for emulsion polymerization of this form do not need to "have a carbonyl group, a formyl group and an alkenyl group in the same or different molecules", and other than that, it is the same as the specific form and suitable form of the PVA contained in the aqueous solution described in the first form of the present invention. The method for manufacturing PVA is also as described above.
[0193] The use, components contained, etc. of the dispersant for emulsion polymerization according to the second aspect of the present invention are the same as those of the dispersant for emulsion polymerization according to the first aspect of the present invention.
[0194] <Water-based emulsion>
[0195] One embodiment of the present invention is an aqueous emulsion, which includes a polymer and the aforementioned emulsion polymerization dispersant, wherein the polymer includes a structural unit derived from at least one selected from an ethylenically unsaturated monomer and a diene monomer. The polymer containing a structural unit derived from at least one selected from an ethylenically unsaturated monomer and a diene monomer is a dispersoid of the aqueous emulsion. The dispersion medium of the aqueous emulsion includes water. The dispersion medium of the aqueous emulsion can be water. The aqueous emulsion may further include components other than the aforementioned polymer and dispersion medium. From the viewpoint of stability, the pH of the aqueous emulsion is preferably above 5 and below 6.
[0196] In addition, the aqueous emulsion may contain a dispersion stabilizer other than the aforementioned emulsion polymerization dispersant. As a dispersion stabilizer, a surfactant is suitably used. As the surfactant, there is no particular limitation, and for example, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants and high molecular compounds (polymer surfactants) with surface activity can be used. As anionic surfactants, for example, alkylnaphthalene sulfonates, dialkyl sulfosuccinates, alkyldiphenyl ether sulfonates, naphthalenesulfonic acid-formaldehyde condensates, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkylphenyl ether sulfates, etc. can be listed. As cationic surfactants, for example, quaternary ammonium salts such as alkylamine salts, lauryltrimethylammonium chloride, and distearyldimethylammonium chloride can be listed. As nonionic surfactants, for example, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid monoglycerides, polyethylene glycol fatty acid esters, polyoxyethylene alkylamines, etc. can be listed. As amphoteric surfactants, for example, alkyl betaines, amine oxides, imidazolium betaines, etc. can be listed. As polymer surfactants, basically, as long as they have a hydrophilic group and a hydrophobic group in the molecule, for example, various carboxylic acid-type polymer surfactants, oxyethylene-oxypropylene block polymers (プルロニック (registered trademark) type surfactants), other PVAs other than the aforementioned PVA, cellulose derivatives such as hydroxyethyl cellulose, etc. can be listed. Among these, dialkyl sulfosuccinates, alkyl diphenyl ether sulfonates, polyoxyethylene alkyl ether sulfates, lauryl trimethyl ammonium chloride, polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, other PVAs, hydroxyethyl cellulose, etc. are preferably used.
[0197] As one or more monomers selected from ethylenically unsaturated monomers and diene monomers, for example, olefin monomers such as ethylene, propylene, and isobutylene; halogenated olefin monomers such as vinyl chloride, vinyl fluoride, vinylidene chloride, and vinylidene fluoride; vinyl ester monomers such as vinyl formate, vinyl acetate, vinyl propionate, and vinyl versatate; (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, and (meth)acrylic acid. (Meth)acrylate monomers such as 2-hydroxyethyl (meth)acrylate; (meth)acrylamide monomers such as dimethylaminoethyl (meth)acrylate and its quaternary products, (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, (meth)acrylamide-2-methylpropanesulfonic acid and its sodium salt; styrene monomers such as styrene, α-methylstyrene, p-styrenesulfonic acid and their sodium salts and potassium salts; diene monomers such as butadiene, isoprene, chloroprene; N-vinyl pyrrolidone, etc. It should be noted that in this specification, "(meth)acrylic acid" refers to acrylic acid and methacrylic acid.
[0198] Among the ethylenically unsaturated monomers and the diene monomers, at least one selected from the group consisting of vinyl ester monomers, (meth)acrylate monomers, styrene monomers, and diene monomers is preferred.
[0199] Furthermore, it is preferred to use (meth)acrylate monomers, styrene monomers, and mixtures of two or more of these monomers, and other monomers copolymerizable therewith may be contained as a small amount of component (e.g., 0 to 40% by mass). As the monomer constituting the (meth)acrylate polymer, it is more preferred to use an alkyl acrylate having an alkyl group with 1 to 8 carbon atoms, an alkyl methacrylate having an alkyl group with 1 to 8 carbon atoms, or a mixture thereof.
[0200] <Method for producing aqueous emulsion>
[0201] One embodiment of the present invention is a method for producing an aqueous emulsion, comprising: subjecting at least one monomer selected from an ethylenically unsaturated monomer and a diene monomer to emulsion polymerization in the presence of the aforementioned emulsion polymerization dispersant. The aqueous emulsion obtained in this manner has a low content of aggregates containing coarse particles and excellent mechanical stability.
[0202] In the aforementioned manufacturing method, when the aforementioned dispersant for emulsion polymerization is added to the polymerization system, there is no particular limitation on the method of adding and adding the dispersant. Examples include a method of adding the dispersant for emulsion polymerization to the polymerization system at the initial stage and a method of adding the dispersant continuously during the polymerization. Among them, from the viewpoint of increasing the grafting rate of PVA to the emulsion dispersoid, the method of adding the dispersant for emulsion polymerization to the polymerization system at the initial stage is preferred.
[0203] The amount of the dispersant for emulsion polymerization used during emulsion polymerization is preferably 0.2 to 40 parts by mass, more preferably 0.3 to 20 parts by mass, and even more preferably 0.5 to 15 parts by mass, relative to 100 parts by mass of at least one monomer selected from ethylenically unsaturated monomers and diene monomers. By making the amount of the dispersant for emulsion polymerization within the above range, there is a tendency that the aggregation of the dispersed particles of the aqueous emulsion can be further suppressed, the polymerization stability is improved, and the viscosity of the polymerization system can be suppressed from becoming too high, the polymerization can be carried out more uniformly, and the heat removal of the polymerization heat becomes better.
[0204] In the emulsion polymerization carried out using a dispersant for emulsion polymerization, as a polymerization initiator, a water-soluble single initiator or a water-soluble redox initiator commonly used in emulsion polymerization is used. For example, as a single initiator, hydrogen peroxide, persulfate (potassium, sodium or ammonium salt) and the like can be listed. As a redox initiator, an initiator obtained by combining a peroxide with a metal ion; an initiator obtained by combining a peroxide, a metal ion and a reducing substance can be listed. As the aforementioned peroxide, hydroperoxides such as hydrogen peroxide, isopropylbenzene hydroperoxide, and tert-butyl hydroperoxide can be listed; persulfate (potassium, sodium or ammonium salt), tert-butyl peracetate, perester (tert-butyl perbenzoate) can be listed. As the aforementioned metal ion, Fe 2+ Cr 2+ 、V 2+ 、Co 2+ 、Ti 3+ , Cu + Examples of the reducing substance include sodium bisulfite, sodium bicarbonate, tartaric acid, Rongalite, 1-ethyl-ascorbic acid, and ascorbic acid.
[0205] The dispersion medium in the emulsion polymerization is preferably an aqueous medium with water as the main component. The aqueous medium with water as the main component may contain a water-soluble organic solvent (alcohols, ketones, etc.) that can be miscible with water in any proportion. Here, "aqueous medium with water as the main component" refers to a dispersion medium containing more than 50% by mass of water. From the viewpoint of cost and environmental burden, the dispersion medium is preferably an aqueous medium containing more than 90% by mass of water, more preferably water.
[0206] In the emulsion polymerization, other protective colloids such as polyacrylic acid or polymethacrylic acid and salts thereof; polyvinyl alkyl ethers; copolymers of vinyl acetate and acrylic acid, methacrylic acid or maleic anhydride and saponified products thereof; lower alkyl vinyl ether-maleic anhydride copolymers; cellulose derivatives such as alkyl cellulose, hydroxyalkyl cellulose, alkyl hydroxyalkyl cellulose, carboxymethyl cellulose; starch derivatives such as alkyl starch, carboxymethyl starch, oxidized starch; gum arabic, tragacanth; polyalkylene glycol, etc. may be added during or after the polymerization to give the desired properties to the emulsion, within the range that the effects of the present invention are not impaired. In addition, auxiliary agents such as liquid property regulators, monohydric alcohols or polyhydric alcohols, plasticizers, defoaming agents, etc., which are conventionally used in emulsion polymerization, may also be used in combination during or after the polymerization.
[0207] <Laminate>
[0208] One embodiment of the present invention is a laminated body, which comprises a substrate and a layer formed of the aqueous emulsion. The layer formed of the aqueous emulsion may be a layer formed by drying the aqueous emulsion. The laminated body may comprise a substrate and a layer formed of a coating agent containing the aqueous emulsion.
[0209] Another embodiment of the present invention is a laminate comprising a substrate and a layer containing the dispersant for emulsion polymerization. The layer formed of the aqueous emulsion is an example of a layer containing the dispersant for emulsion polymerization.
[0210] A suitable embodiment of the laminate is a coated paper formed by coating a coating agent containing the aforementioned aqueous emulsion on paper as a substrate. The coating agent may be the aforementioned aqueous emulsion. As the substrate paper used in the coated paper, known paper or synthetic paper obtained by papermaking chemical pulps such as hardwood kraft pulp and softwood kraft pulp, GP (woodchip pulp), RGP (refined machine pulp), TMP (thermomechanical pulp) and the like may be used. In addition, as the aforementioned paper, high-quality paper, medium-quality paper, alkaline paper, glassine, semi-glassine, or cardboard, white cardboard used for corrugated cardboard, building materials, abaca cardboard, white board, particle board, etc. may also be used. The basis weight of the aforementioned paper is not particularly limited as long as it is adjusted according to the application, and is generally 10 to 500 g / m 2 Below, preferably 40 to 200 g / m 2 It should be noted that the paper used in the aforementioned coated paper may contain papermaking auxiliary chemicals such as organic pigments or inorganic pigments, paper strength enhancers, sizing agents, and yield improvers. In addition, the paper used in the aforementioned coated paper may be subjected to various surface treatments.
[0211] The coating amount of the coating agent can be arbitrarily selected according to the properties of the paper to be coated, and is usually preferably 0.1 to 30 g / m2 in terms of solid content.2 The coating agent may be applied to the surface of the paper or may be impregnated into the inside. In the former case, the coating agent may be applied to one side of the paper or may be applied to both sides.
[0212] As a method for applying the coating agent to paper, there are transfer methods such as SYM-SIZER and gate roll coater; and impregnation methods such as size press. From the viewpoint of easier formation of the coating layer, the transfer method is preferred. On the other hand, since the coating agent easily forms a film, even in the case of the impregnation method, the aforementioned coating agent is inhibited from penetrating into the interior of the paper, and a coating layer is effectively formed near the surface. Therefore, on the basis of reducing the coating amount, it is also easy to dry and the cost is reduced. The temperature of the aforementioned coating agent during coating is usually room temperature to 100°C.
[0213] The paper coated with the coating solution can be dried by a known method, such as hot air, infrared rays, a heated cylinder, or a combination thereof. The drying temperature is usually room temperature to 120°C. The barrier properties can be further improved by conditioning the moisture of the dried coated paper and subjecting it to a calender treatment. As calender treatment conditions, the roll temperature is usually room temperature to 100°C, and the roll line pressure is 20 to 300 kg / cm.
[0214] The coated paper may have a layer other than the layer formed of the aqueous emulsion or the layer containing the dispersant for emulsion polymerization.
[0215] Coated paper can also be used as special paper such as release paper, oil-resistant paper, thermal paper, inkjet paper, pressure-sensitive paper, air-barrier paper, and other barrier papers. Among them, it can be preferably used as release paper and oil-resistant paper.
[0216] Example
[0217] The present invention is specifically described by the following examples, but the present invention is not limited to these examples at all. It should be noted that each measurement method in the following examples and comparative examples is shown below.
[0218] [Viscosity average degree of polymerization of PVA]
[0219] The viscosity average polymerization degree of PVA was measured in accordance with JIS K6726: 1994. Specifically, when the saponification degree of PVA is less than 99.5 mol%, the PVA is saponified until the saponification degree reaches 99.5 mol% or more, and the obtained PVA is measured in water at 30°C, and the intrinsic viscosity [η] (liter / g) obtained thereby is used to calculate the viscosity average polymerization degree using the following formula.
[0220] Viscosity average degree of polymerization = ([η] × 10 4 / 8.29) (1 / 0.62)
[0221] [Saponification degree of PVA]
[0222] The saponification degree of PVA was determined by the method described in JIS K6726:1994.
[0223] [Carbonyl content of PVA]
[0224] conduct 1 H-NMR measurement was used to calculate the carbonyl content of PVA. The sample was Soxhlet washed with methyl acetate for 10 hours and vacuum dried at 40°C for 16 hours to remove impurities before being subjected to measurement. The sample prepared in the form of a 1% by mass DMSO-d6 solution (with 0.03% by mass tetramethylsilane added as an internal standard) was measured at 400 MHz (80°C, 256 cumulative times). Among the methyl groups in the main chain of PVA, the peak of CH connected to an OH group appears at 3.8 to 4.0 ppm (integral value [M]), and the peak of CH connected to an OAc group appears at 4.2 to 4.6 ppm (integral value [N]). In addition, the peak of the methylene group adjacent to the formyl group and the carbonyl group appears at 2.3 to 2.5 ppm (integral value [O]). Furthermore, the peak of the proton constituting the formyl group appears at 9.5 to 10.0 ppm (integral value [P]). The carbonyl group content of PVA was determined by the following formula as a value relative to the structural units (vinyl alcohol units and vinyl ester units) derived from the vinyl alcohol monomer.
[0225] Carbonyl content (mol%) = [{([O] / 2)-[P]} / ([M]+[N])]×100
[0226] [Alkenyl content of PVA]
[0227] conduct 1 H-NMR measurement, calculate the content of alkenyl (vinyl) in PVA. The sample was Soxhlet washed with methyl acetate for 10 hours, and vacuum dried at 40°C for 16 hours to remove impurities, and then provided for measurement. A sample prepared in the form of a 1% by mass DMSO-d6 solution (0.03% by mass tetramethylsilane was added as an internal standard) was measured at 400 MHz (80°C, 256 times cumulatively). Among the methyl groups in the main chain of PVA, the peak of CH connected to the OH group appears at 3.8 to 4.0 ppm (integral value [M]), and the peak of CH connected to the OAc group appears at 4.2 to 4.6 ppm (integral value [N]). In addition, the peak of one proton constituting the vinyl group in the alkenyl group (H at position 1 in the vinyl group; CH2=C"H"-) appears at 5.7 to 6.0 ppm (integral value [Q]). The content of the alkenyl group of PVA is calculated relative to the value of the structural unit (vinyl alcohol unit and vinyl ester unit) derived from the vinyl alcohol monomer using the following formula.
[0228] Alkenyl content (mol%) = {[Q] / ([M]+[N])}×100
[0229] [Formyl content of PVA]
[0230] conduct 1 H-NMR measurement, calculate the content of formyl group in PVA. The sample was Soxhlet washed with methyl acetate for 10 hours, and vacuum dried at 40°C for 16 hours to remove impurities, and then provided for measurement. The sample prepared in the form of 1 mass % DMSO-d6 solution (0.03 mass % tetramethylsilane added as internal standard) was measured at 400 MHz (80°C, cumulative 256 times). Among the methyl groups in the main chain of PVA, the peak of CH connected to the OH group appears at 3.8 to 4.0 ppm (integral value [M]), and the peak of CH connected to the OAc group appears at 4.2 to 4.6 ppm (integral value [N]). The peak of the proton constituting the formyl group appears at 9.5 to 10.0 ppm (integral value [P]). The content of formyl group in PVA is calculated relative to the value of the structural unit (vinyl alcohol unit and vinyl ester unit) derived from the vinyl alcohol monomer using the following formula.
[0231] Formyl content (mol%) = {[P] / ([M]+[N])}×100
[0232] [Determination of Na content]
[0233] The Na content was determined by atomic absorption spectrometry as follows. 1.0 parts by mass of PVA was carbonized at 650°C, and then 2.0 parts by mass of hydrochloric acid was added and heated at 150°C for 3 minutes. The solution was dissolved in ion exchange water to prepare 50 mL of an aqueous solution. The atomic absorption of the aqueous solution was measured, and the Na content was calculated using a separately prepared standard curve.
[0234] [Water-insoluble ingredients]
[0235] The water-insoluble components of PVA are determined as follows. A 500mL flask equipped with a stirrer and a reflux condenser is prepared in a water bath set to 20°C, 285g of distilled water is added to the flask, and stirring is started at 300rpm. 15g of PVA particles are weighed and slowly added to the flask. After all the PVA particles (15g) are added, it takes 30 minutes to raise the temperature of the water bath to 90°C, thereby dissolving the PVA particles and obtaining a PVA solution. After the temperature of the water bath reaches 90°C, the solution is further dissolved while stirring at 300rpm for 60 minutes. Thereafter, the PVA solution is used to filter the undissolved and residual PVA particles (undissolved particles) using a metal filter with a mesh of 63μm. Next, the filter is thoroughly washed with warm water at 90°C to remove the PVA solution attached to the filter. After only undissolved particles remain on the filter, the filter is dried in a 120°C heating dryer for 1 hour. The mass of the filter after drying was compared with the mass of the filter before filtration to calculate the mass of the insoluble particles. The ratio of the mass of the insoluble particles to the mass of PVA (15 g) initially added to the water was defined as the water-insoluble content (ppm).
[0236] [Manufacturing Example A1] (Manufacturing of PVA-A1)
[0237] 1600 parts by mass of vinyl acetate and 16.0 parts by mass of 7-octenal were added to a reactor equipped with a stirrer, a reflux condenser, a nitrogen inlet pipe, and a polymerization initiator addition port, and the system was purged with nitrogen for 30 minutes while nitrogen bubbling. The temperature of the reactor was started, and when the internal temperature reached 70°C, 0.28 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) was added to start polymerization. After polymerization at 70°C for 4 hours, the polymerization was stopped by cooling. The solid content concentration at the time of polymerization termination was 39.7% by mass and the polymerization rate was 40%. Next, unreacted monomers were removed while adding methanol at any time under reduced pressure at 30°C to obtain a methanol solution of a vinyl ester polymer (concentration of 35.2% by mass). Next, 2.1 parts by mass of a 10% by mass methanol solution of sodium hydroxide and 1.2 parts by mass of ion exchange water were added to 116.8 parts by mass of a methanol solution of a vinyl ester polymer prepared by further adding methanol to the methanol solution (30 parts by mass of the aforementioned polymer in the solution), and saponification was performed at 40°C (the aforementioned polymer concentration in the saponified solution was 25% by mass, the water content of the saponified solution was 1% by mass, and the molar ratio of sodium hydroxide to the vinyl acetate unit in the aforementioned polymer was 0.015). A gel-like substance was generated about 10 minutes after the addition of the methanol solution of sodium hydroxide, so it was crushed with a pulverizer and further placed at 40°C for 1 hour for saponification. Thereafter, 120 parts by mass of methanol was added, and the mixture was placed at 40°C for washing for 30 minutes. After repeating this washing operation twice, the liquid was removed, and the obtained white solid was vacuum dried at 40°C for 16 hours to obtain PVA (PVA-A1). The analysis results of PVA-A1 are shown in Table 2.
[0238] [Manufacturing Examples A2, A3, A5, and A6] (Manufacturing of PVA-A2, A3, A5, and A6)
[0239] The PVAs of Manufacturing Examples A2, A3, A5, and A6 (PVA-A2, A3, A5, and A6) were manufactured by the same method as in Manufacturing Example 1, except that the amount of vinyl acetate fed, the amount of methanol used, the type, amount, and polymerization temperature of the monomer (a) used during polymerization, the concentration of the vinyl ester polymer during saponification, and the molar ratio of sodium hydroxide to the vinyl acetate unit were changed as shown in Table 1. As described in Table 1, Manufacturing Example A6 was manufactured by using the monomer (a) and the monomer (b) together. The analysis results of PVA-A2, A3, A5, and A6 are shown in Table 2.
[0240] [Manufacturing Example A4] (Manufacturing of PVA-A4)
[0241] 1600 parts by mass of vinyl acetate, 5.0 parts by mass of 7-octenal and 200 parts by mass of methanol were added to a reactor equipped with a stirrer, a reflux condenser, a nitrogen inlet pipe and a polymerization initiator addition port, and the system was purged with nitrogen for 30 minutes while nitrogen bubbling. The temperature of the reactor was started, and when the internal temperature reached 60°C, 0.1 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) was added to start polymerization. After polymerization at 60°C for 4 hours, the polymerization was stopped by cooling. The solid content concentration at the time of polymerization termination was 26.7% by mass and the polymerization rate was 30%. Next, unreacted monomers were removed while adding methanol at any time under reduced pressure at 30°C to obtain a methanol solution of a vinyl ester polymer (concentration of 30.2% by mass). Next, 1.3 parts by mass of a 10% by mass methanol solution of sodium hydroxide and 1.2 parts by mass of ion exchange water were added to 117.7 parts by mass of a methanol solution of a vinyl ester polymer prepared by further adding methanol to the methanol solution (30 parts by mass of the aforementioned polymer in the solution), and saponification was performed at 40°C (the aforementioned polymer concentration in the saponified solution was 25% by mass, the water content of the saponified solution was 1% by mass, and the molar ratio of sodium hydroxide to the vinyl acetate unit in the aforementioned polymer was 0.009). A gel-like substance was generated about 10 minutes after the addition of the methanol solution of sodium hydroxide, so it was crushed with a pulverizer and further placed at 40°C for 1 hour for saponification. Thereafter, 120 parts by mass of methanol was added and the mixture was placed at 40°C for washing for 30 minutes. After repeating the washing operation twice, the liquid was removed, and the obtained white solid was vacuum dried at 40°C for 16 hours to obtain PVA (PVA-A4). The analysis results of PVA-A4 are shown in Table 2.
[0242] [Manufacturing Example A7] (Manufacturing of PVA-A7)
[0243] PVA (PVA-A7) was produced by the same method as in Production Example A4 except that the monomer (a) was not used, and the polymerization conditions such as the amount of vinyl acetate charged, the amount of methanol used, the polymerization temperature, the concentration of the vinyl ester polymer during saponification, and the molar ratio of sodium hydroxide to the vinyl acetate unit were changed as shown in Table 1. The analysis results of PVA-A7 are shown in Table 2.
[0244] [Manufacturing Example A8] (Manufacturing of PVA-A8)
[0245] The raw material PVA (c) was produced by the same method as in Production Example A7, except that the feeding amount of vinyl acetate, the amount of methanol, the polymerization conditions such as the polymerization temperature, the concentration of the vinyl ester polymer during saponification, the molar ratio of sodium hydroxide to the vinyl acetate unit, and the like were changed as shown in Table 1. Next, 80 parts by mass of the raw material PVA (c) was dissolved in 1 L of water at 95°C. Next, it was reacted with 0.5 parts by mass of 10-undecene aldehyde at 90°C for 1 hour under acidic conditions (sulfuric acid, pH = 1.5). After the reaction was completed, the pH was adjusted to 7 using sodium hydroxide. The reaction solution was dried to obtain PVA (PVA-A8). The analysis results of PVA-A8 are shown in Table 2.
[0246] [Manufacturing Example A9] (Manufacturing of PVA-A9)
[0247] Using the raw material PVA (c) manufactured by the same method as in Manufacturing Example A8, 20 parts by mass of the raw material PVA (c) was dissolved in 400 mL of N-methylpyrrolidone at 120°C. Thereafter, the solution was cooled to room temperature while stirring. Next, 0.3 parts by mass of 10-undecanoyl chloride dissolved in 10 mL of N-methylpyrrolidone was added under a nitrogen atmosphere. After 15 minutes, 3.5 parts by mass of pyridine and 0.5 parts by mass of dimethylaminopyridine were added and reacted at room temperature for 48 hours. The reaction solution was added dropwise to acetone to recover the precipitate. Furthermore, reprecipitation and purification were carried out using water / acetone, and the recovered precipitate was vacuum dried for 8 hours to obtain PVA (PVA-A9). The analysis results of PVA-A9 are shown in Table 2.
[0248] [Manufacturing Example A10] (Manufacturing of PVA-A10)
[0249] Using the raw material PVA (c) produced by the same method as in Production Example A8, a solution was prepared by dissolving 6 parts by mass of itaconic acid and 0.3 parts by mass of propyl gallate in 150 parts by mass of methanol, 100 parts by mass of the raw material PVA (c) was added thereto to make it swell, and then the methanol was removed under reduced pressure. Thereafter, the obtained mixed powder was heat-treated at a temperature of 105° C. for 4 hours to obtain PVA (PVA-A10). The analysis results of PVA-A10 are shown in Table 2.
[0250] [Manufacturing Example A11] (Manufacturing of PVA-A11)
[0251] 1000 parts by mass of vinyl acetate, 600 parts by mass of methanol, and 8.8 parts by mass of propene diacetate were added to a reactor equipped with a stirrer, a reflux condenser, a nitrogen inlet, a chain transfer agent addition port, and a polymerization initiator addition port. The system was purged with nitrogen for 30 minutes while nitrogen bubbling was performed. The temperature of the reactor was started, and when the internal temperature reached 60°C, 3.8 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) was added to start polymerization. A methanol solution of propene diacetate (concentration of 50% by mass) was added dropwise to the reactor. The solution was added dropwise (total amount of addition was 15.2 parts by mass) while maintaining a constant composition ratio with vinyl acetate in the polymerization solution. After polymerization at 60°C for 10 hours, the polymerization was stopped by cooling. The solid content concentration at the time of stopping the polymerization was 49.0% by mass, and the polymerization rate was 80%. Next, PVA (PVA-A11) was obtained by the same method as in Production Example 1 except that saponification conditions such as the concentration of the vinyl ester polymer during saponification and the molar ratio of sodium hydroxide to vinyl acetate units were changed as shown in Table 1. The analysis results of PVA-A11 are shown in Table 2.
[0252]
[0253] [Table 2]
[0254]
[0255] [Example A1] (Preparation of aqueous solution)
[0256] PVA-A1 obtained in Production Example A1 was added to stirred water and heated to 95° C. to dissolve in water to prepare an aqueous solution having a concentration of 6% by mass (1560 parts by mass of water relative to 100 parts by mass of PVA).
[0257] The aqueous solution prepared above was used as a coating agent to prepare a release paper base paper by the following method. The stability of the coating agent (aqueous solution), coating unevenness of the release paper base paper, air permeability (air resistance), silicone curing property, and adhesion of the release layer were evaluated by the following method. The results are shown in Table 3.
[0258] (Aqueous solution stability)
[0259] The state of the aqueous solution after being left at 40° C. for 7 days was observed, and the state changes before and after storage were evaluated according to the following indexes. If it was A to B, it was judged that the storage stability was excellent.
[0260] A: No separation or sedimentation occurs
[0261] B: Slight separation and sedimentation were observed, but the product has fluidity
[0262] C: Separation and sedimentation are confirmed. Or there is no fluidity
[0263] (Manufacturing of release paper base paper)
[0264] The coating agent was applied using a wire rod in an amount of about 0.7 g / m2 in dry weight. 2 The coated paper was coated on a glass paper with an air permeability of 100 sec. After coating, the coated paper was dried at 100°C for 5 minutes. The coated paper was calendered at 70°C and 400 kg / cm 2 The obtained coated paper was treated twice to obtain a base paper for release paper.
[0265] (Evaluation of coating unevenness)
[0266] Cut the above release paper base into a size of 1 cm in length and 2 cm in width, add a drop of 1 / 200 equivalent iodine aqueous solution, and observe the surface of the coated paper. Among the coated surfaces, the part bearing the coating liquid is dyed into blue-purple, and the part not bearing the coating liquid is dyed into red-purple. Based on this difference, the coating unevenness is judged according to the following criteria. If it is A to B, it is judged to be excellent in coating properties.
[0267] A: Even
[0268] B: Local unevenness
[0269] C: Overall unevenness
[0270] (Determination of air permeability)
[0271] The air permeability of the release paper base paper was measured using a Wangyan smoothness air permeability tester in accordance with JIS P8117 and evaluated according to the following indexes: If it is A to B, it is judged to be excellent in air permeability resistance.
[0272] A: More than 50,000 seconds
[0273] B: more than 1000 seconds and less than 50000 seconds
[0274] C: Less than 1000 seconds
[0275] (Evaluation of Silicone Curability)
[0276] LTC1056L manufactured by Toray Daw Coning Co., Ltd. was used as the addition silicone, and SRX212 was used as the platinum catalyst. The coating solution was mixed with a blade coater so that the ratio of the addition silicone to platinum was 100 / 0.007, and the coating solid content was 1.5 g / m 2The obtained release paper base is coated in the manner of . By doing so, a silicone layer is formed on the release paper base. Then, heat treatment is performed at 110°C, and the time until the silicone is cured is measured and evaluated according to the following indicators. Here, the time until the silicone is cured refers to the time (seconds) required until the silicone layer is completely no longer peeled off after rubbing the silicone layer 10 times with fingers at a prescribed time interval. If it is A to B, it is judged that the silicone curing property is excellent.
[0277] A: Less than 60 seconds
[0278] B: more than 60 seconds and less than 120 seconds
[0279] C: 120 seconds or more
[0280] (Evaluation of Adhesion of Peel Layer)
[0281] On the release paper base, LTC1056L manufactured by Toray Daw Coning Co., Ltd. was used as the addition type silicone, and SRX212 was used as the platinum catalyst. The coating liquid was mixed in a ratio of 100 / 0.009 of the addition type silicone and platinum by a blade coater so that the coating solid content was 1.5 g / m 2 The obtained release paper base paper was coated with the release paper in the manner of , and heat treated at 110°C for 90 seconds to obtain a release paper having a release layer (silicone layer) formed on the release paper base paper. The obtained release paper was evaluated according to the following indicators. If it was A to B, it was judged to be excellent in adhesion.
[0282] A: After leaving it at 40°C and 90% RH for one week, the silicone layer was strongly rubbed with fingers. As a result, the silicone layer did not peel off. After leaving it at the same conditions for another week, the silicone layer was strongly rubbed with fingers. As a result, the silicone layer did not peel off.
[0283] B: After leaving it at 40°C and 90% RH for one week, the silicone layer was strongly rubbed with fingers. As a result, the silicone layer did not peel off. However, after leaving it at the same conditions for another week, the silicone layer was strongly rubbed with fingers, and the silicone layer peeled off.
[0284] C: After being left at 40°C and 90% RH for one week, the silicone layer was strongly rubbed with fingers. As a result, the silicone layer peeled off.
[0285] [Examples A2 to A6, Comparative Examples A1 to A4]
[0286] The aqueous solution (coating agent) was prepared by the same method as in Example A1 except that the type of PVA was changed to the content of Table 3, and the release paper base paper was prepared. The aqueous solution stability of the obtained aqueous solution (coating agent), and the coating unevenness, air permeability, silicone curing property and adhesion of the release paper base paper were evaluated by the same method as in Example A1. The results are shown in Table 3.
[0287] [Table 3]
[0288] PVA Aqueous solution stability Uneven coating Breathability Silicone curing Adhesion Example A1 PVA-A1 A A A A A Example A2 PVA-A2 A A A A A Example A3 PVA-A3 A A B A A Example A4 PVA-A4 A A A B B Example A5 PVA-A5 A A A A A Example A6 PVA-A6 A A B A A Comparative Example A1 PVA-A7 A A B C C Comparative Example A2 PVA-A8 C B B C B Comparative Example A3 PVA-A9 A A C C C Comparative Example A4 PVA-A10 A C C C B
[0289] As shown in Table 3, it can be seen that the aqueous solution of the coating agent containing the aqueous solution of the vinyl alcohol polymer having a carbonyl group, a formyl group and an alkenyl group in the same or different molecules has excellent aqueous solution stability and less coating unevenness during coating. It can also be seen that the air permeability of the obtained release paper base paper is high, and the silicone curing property and the adhesion of the release layer are also good (Examples A1 to A6). In particular, when the carbonyl content of PVA is 0.05 mol% or more, the alkenyl content is 0.04 mol% or more, and the formyl content is 0.1 mol% or more, the silicone curing property and the adhesion of the release layer are particularly excellent (Examples A1 to A3, A5, A6). On the other hand, when PVA-A7 without a carbonyl group, an alkenyl group and a formyl group is used, the silicone curing property and the adhesion of the release layer are significantly poor (Comparative Example A1). In addition, when PVA having only an alkenyl group is used, the aqueous solution stability is poor, and further, the silicone curing property and the adhesion of the release layer are also insufficient (Comparative Examples A2 to A4).
[0290] [Example A7] (Preparation of Adhesive)
[0291] PVA-A1 obtained in Preparation Example A1 was added to stirring water and heated to 95°C to dissolve in water to prepare an aqueous solution with a concentration of 15% by mass (567 parts by mass of water relative to 100 parts by mass of PVA) and used as an adhesive. The initial adhesion and water-resistant adhesion were evaluated by the following methods.
[0292] (Initial Adhesion)
[0293] In an atmosphere of 20°C and 65% RH, the adhesive was applied to kraft paper using a No. 6 wire rod, and kraft paper was further attached thereto, and then compacted three times using a manual roller. After compaction, the time until the kraft paper was completely broken without being peeled off by hand was measured, and the evaluation was performed according to the following criteria. If it was A to B, it was judged that the initial adhesion was excellent. The results are shown in Table 4.
[0294] A: Less than 3 seconds, the kraft paper is completely damaged
[0295] B: 3 seconds or more and less than 5 seconds, the kraft paper is completely damaged
[0296] C: 5 seconds or more and less than 10 seconds, the kraft paper is completely damaged
[0297] D: After 10 seconds, the kraft paper is completely damaged.
[0298] (Water-resistant adhesion)
[0299] In an atmosphere of 20°C and 65% RH, the adhesive was applied to kraft paper using a No. 6 wire rod, and after further pasting kraft paper thereon, it was compacted 3 times using a manual roller. After the kraft paper was dried at 100°C for 5 minutes, it was cured for 24 hours in an atmosphere of 20°C and 65% RH, and then immersed in water at 30°C for 30 seconds. After gently wiping off the moisture of the kraft paper containing water using filter paper, the 180°C peel strength of the adhesive layer was measured using Autograph and evaluated according to the following indicators. If it is A to B, it is judged to be excellent in water-resistant adhesion. The results are shown in Table 4.
[0300] A: The kraft paper material is damaged
[0301] B: 1kg / cm 2 above
[0302] C: less than 1kg / cm 2
[0303] [Examples A8 to A12, Comparative Examples A5 and A6]
[0304] An adhesive was prepared by the same method as in Example A7 except that the type of PVA was changed to that shown in Table 4. The initial adhesion and water-resistant adhesion of the obtained adhesive were evaluated by the same method as in Example A7. The results are shown in Table 4.
[0305] [Table 4]
[0306] PVA Initial adhesion Water-resistant adhesion Example A7 PVA-A1 A A Example A8 PVA-A2 A A Embodiment A9 PVA-A3 A B Embodiment A10 PVA-A4 A B Embodiment A11 PVA-A5 A A Example A12 PVA-A6 B A Comparative Example A5 PVA-A7 C C Comparative Example A6 PVA-A11 C B
[0307] As shown in Table 4, the adhesive containing the aqueous solution of the vinyl alcohol polymer having a carbonyl group, a formyl group and an alkenyl group in the same or different molecules has good initial adhesion and water-resistant adhesion (Examples A7 to A12). In particular, when the saponification degree of PVA is 75 mol% or more, the carbonyl content is 0.05 mol% or more, the alkenyl content is 0.04 mol% or more, and the formyl content is 0.1 mol% or more, the water-resistant adhesion is particularly excellent (Examples A7, A8, A11, A12). On the other hand, when PVA-A7, which does not have a carbonyl group, an alkenyl group and a formyl group, is used, the initial adhesion and water-resistant adhesion are significantly poor (Comparative Example A5). In addition, when PVA-A11, which only has a formyl group, is used, the initial adhesion is poor (Comparative Example A6).
[0308] [Manufacturing Example B1] (Manufacturing of PVA-B1)
[0309] 1600 parts by mass of vinyl acetate and 35.0 parts by mass of 7-octenal were added to a reactor equipped with a stirrer, a reflux condenser, a nitrogen inlet pipe and a polymerization initiator addition port, and the system was purged with nitrogen for 30 minutes while nitrogen bubbling. The temperature of the reactor was started, and when the internal temperature reached 60°C, 2.4 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) was added to start polymerization. After polymerization at 60°C for 3 hours, the polymerization was stopped by cooling. The solid content concentration at the time of polymerization termination was 44.3% by mass and the polymerization rate was 45%. Next, unreacted monomers were removed while adding methanol at any time under reduced pressure at 30°C to obtain a methanol solution of a vinyl ester polymer (concentration of 38.2% by mass). Next, 6.8 parts by mass of a 5% by mass methanol solution of sodium hydroxide and 1.84 parts by mass of ion exchange water were added to 191.3 parts by mass of a methanol solution of a vinyl ester polymer prepared by further adding methanol to the methanol solution (60 parts by mass of the aforementioned polymer in the solution), and saponification was performed at 40°C (the concentration of the aforementioned polymer in the saponified solution was 30% by mass, the water content of the saponified solution was 1% by mass, and the molar ratio of sodium hydroxide to the vinyl acetate unit in the aforementioned polymer was 0.012). A gel-like substance was generated about 10 minutes after the addition of the methanol solution of sodium hydroxide, so it was crushed with a pulverizer and further placed at 40°C for 1 hour for saponification. Thereafter, 200 parts by mass of methanol was added and the solution was placed at 40°C for washing for 30 minutes. After repeating this washing operation twice, the solution was deliquified, and the obtained white solid was vacuum dried at 40°C for 16 hours to obtain PVA (PVA-B1). The physical properties of PVA-B1 are shown in Table 6.
[0310] [Manufacturing Examples B2 to B9] (Manufacturing of PVA-B2 to PVA-B9)
[0311] PVA (PVA-B2 to PVA-B7) was produced by the same method as that for producing PVA-B1, except that the polymerization conditions such as the amount of vinyl acetate fed, the type and amount of aldehyde used in the polymerization, the concentration of the vinyl ester polymer in the saponification, and the molar ratio of sodium hydroxide to the vinyl acetate unit were changed as shown in Table 5. PVA-B4 was produced by using aldehyde (a) and chain transfer agent (b) at the same time as described in Table 5. In addition, PVA-B8 was produced by the same method as that for producing PVA-B1, except that methanol was used in the polymerization and aldehyde (a) was not used. The polymerization conditions such as the amount of vinyl acetate fed, the concentration of the vinyl ester polymer in the saponification, and the molar ratio of sodium hydroxide to the vinyl acetate unit were changed as shown in Table 5. In addition, PVA-B9 was produced by the same method as that of PVA-B1 except that methanol was used in the polymerization, aldehyde (a) was not used, chain transfer agent (b) was used, polymerization conditions such as the amount of vinyl acetate charged, concentration of the vinyl ester polymer in the saponification, and saponification conditions such as the molar ratio of sodium hydroxide to vinyl acetate units were changed as shown in Table 5. The physical properties of each PVA are shown in Table 6.
[0312] [Example B1] (Manufacturing of Em-1)
[0313] In a 1-liter glass container equipped with a reflux condenser, a dropping funnel, a thermometer and a nitrogen blowing port, 20 g of PVA (PVA-B1) was heated and dissolved in 275.0 g of ion exchange water, and the pH was adjusted to 3.5 using dilute sulfuric acid. After the prepared PVA aqueous solution was heated to 75°C while stirring at 200 rpm, 22 g of an aqueous solution of ammonium persulfate with a concentration of 5% by mass and 6.1 g of an aqueous solution of sodium bicarbonate with a concentration of 1% by mass were added. A mixed solution of 100 g of methyl methacrylate, 100 g of 2-ethylhexyl acrylate and 1.0 g of tert-dodecyl mercaptan was added continuously for 3 hours. The polymerization temperature was maintained at 80°C to complete the polymerization, and a reactant with a solid content concentration of 39.8% by mass was obtained. The reactant was adjusted to pH = 5.2 with aqueous ammonia to obtain an aqueous emulsion (Em-1). The following method was used to evaluate the amount of aggregates generated and the mechanical stability of the aqueous emulsion (Em-1). The results are shown in Table 7.
[0314] (Amount of aggregates generated (filtration residue))
[0315] 500 g of the aqueous emulsion was filtered through a 60-mesh standard sieve in accordance with JIS K8801, and the filtration residue was weighed and evaluated as follows: If it was A to C, it was judged that the generation of aggregates was small.
[0316] A: Filtration residue is less than 1.0% by mass
[0317] B: Filtration residue is 1.0 mass % or more and less than 2.5 mass %
[0318] C: Filtration residue is 2.5% by mass or more and less than 5.0% by mass
[0319] D: Filtration residue is 5.0% by mass or more, and filtration is difficult
[0320] (Mechanical stability (solidification rate))
[0321] Using a Malang mechanical stability measuring device, according to JIS K6828, 50 g of the aqueous emulsion was stirred for 10 minutes under a load of 20 kg and 1000 rpm, and then filtered using an 80 mesh metal mesh. The dry mass (g) of the coagulated material on the metal mesh was measured, and the coagulation rate (%) was calculated using the following formula as an indicator of mechanical stability. The smaller the coagulation rate, the better the stability. If the coagulation rate is less than 0.4%, it is judged to be excellent in mechanical stability.
[0322] Coagulation rate (%) = [dry mass of coagulated product / (50×solid content concentration of aqueous emulsion / 100)]×100
[0323] (Manufacture of coated paper for oil-resistant paper)
[0324] The above-mentioned aqueous emulsion is used as a coating agent, and the coating agent is applied to PPC (Plain Paper Copier) paper (high-quality paper) with a basis weight of 70gsm by manual coating using a wire rod. Then, a drum-type rotary dryer is used to dry at 105°C for 5 minutes to produce a coated paper. The coated paper is a laminate having a PPC paper as a substrate and a layer containing an aqueous emulsion. The coating amount converted to the solid content of the coating agent is 5.0gsm (single side). The obtained coated paper is humidified at 20°C and 65%RH for 72 hours. The oil resistance of the humidified coated paper is evaluated by the following KIT test. The results are shown in Table 7.
[0325] (Oil resistance evaluation: KIT test)
[0326] For coated paper, the KIT test of the flat surface of the coated surface is carried out according to TAPPINo.T559cm-02. The evaluation is performed visually. It should be noted that the KIT value of commercially available oil-resistant paper obtained using fluororesin is usually above grade 5, and the oil resistance that does not become a problem in normal use is above grade 5. Therefore, if the oil resistance of the coated paper is above grade 5, it is judged to be excellent in oil resistance. In applications seeking higher oil resistance, it is preferably above grade 7, and more preferably above grade 10.
[0327] [Example B2] (Manufacturing of Em-2)
[0328] Aqueous emulsion (Em-2) and coated paper were prepared and evaluated in the same manner as in Example B1 except that the mass ratio of methyl methacrylate to 2-ethylhexyl acrylate was changed as shown in Table 7. The results are shown in Table 7.
[0329] [Example B3] (Manufacturing of Em-3)
[0330] Aqueous emulsion (Em-3) and coated paper were prepared and evaluated in the same manner as in Example B1 except that methyl methacrylate, 2-ethylhexyl acrylate and styrene were used as monomers in the mass ratio shown in Table 7. The results are shown in Table 7.
[0331] [Examples B4 to B8, Comparative Examples B1 to B3] (Manufacturing of Em-4 to Em-11)
[0332] As shown in Table 7, aqueous emulsions (Em-4 to Em-11) and coated papers were prepared and evaluated in the same manner as in Example B1 except that PVA-B2 to PVA-B9 were used instead of PVA (PVA-B1) in Example B1. The results are shown in Table 7.
[0333]
[0334] [Table 6]
[0335]
[0336] [Table 7]
[0337]
[0338] ※1Methyl methacrylate; MMA, 2-ethylhexyl acrylate; 2-EHA, styrene; St
[0339] ※2 Aqueous emulsion cannot be obtained due to aggregation / caking.
[0340] As shown in Table 7 etc., the generation of aggregates in the aqueous emulsion obtained using a dispersant included in the vinyl alcohol polymer having a carbonyl group, a formyl group and an alkenyl group in the same or different molecules is small, and mechanical stability is also excellent. In addition, the oil resistance of the coated paper manufactured using these aqueous emulsions as coating agents is also excellent.
[0341] Industrial Applicability
[0342] The aqueous solution containing the PVA of the present invention is suitable for coating agents, adhesives, paper processing agents, etc. The dispersant for emulsion polymerization of the present invention is suitable for preparing aqueous emulsions. The aqueous emulsions are suitable for various adhesives, coating matrices, various binders for impregnated paper applications and nonwoven products, various coating agents, etc.
Claims
1. An aqueous solution comprising a vinyl alcohol polymer having a carbonyl group, a formyl group and an alkenyl group in the same or different molecules.
2. The aqueous solution according to claim 1, in, The vinyl alcohol polymer has a structure represented by the following formula (1) including the carbonyl group, [Chemistry 1] In formula (1), m is an integer of 1 to 11.
3. An aqueous solution comprising a vinyl alcohol polymer having a group represented by the following formula (2) at the end of the polymer chain, [Chemistry 2] In formula (2), R 1 It is an alkenyl group.
4. The aqueous solution according to claim 3, in, In the formula (2), R 1 The alkenyl group shown has a methylene group at the terminal end on the carbonyl side.
5. The aqueous solution according to any one of claims 1 to 4, in, The vinyl alcohol-based polymer has tertiary carbon atoms.
6. The aqueous solution according to any one of claims 1 to 5, in, The vinyl alcohol polymer has a structural unit derived from an aliphatic unsaturated aldehyde.
7. The aqueous solution according to claim 6, in, The aliphatic unsaturated aldehyde has 3 to 14 carbon atoms.
8. The aqueous solution according to claim 6 or 7, in, The aliphatic unsaturated aldehyde has a carbon-carbon double bond at the terminal end.
9. The aqueous solution according to any one of claims 1 to 8, in, The concentration of the vinyl alcohol polymer is 0.5 mass % or more and 30 mass % or less. 10 . A coating agent comprising the aqueous solution according to claim 1 .
11. An adhesive comprising the aqueous solution according to any one of claims 1 to 9.
12. A paper processing agent comprising the aqueous solution according to any one of claims 1 to 9.
13. A dispersant for emulsion polymerization, comprising a vinyl alcohol polymer having a carbonyl group, a formyl group and an alkenyl group in the same or different molecules.
14. The dispersant for emulsion polymerization according to claim 13, in, The vinyl alcohol polymer has a structure represented by the following formula (1) including the carbonyl group, [Chemistry 3] In formula (1), m is an integer of 1 to 11.
15. A dispersant for emulsion polymerization, comprising a vinyl alcohol polymer having a group represented by the following formula (2) at the end of the polymer chain, [Chemistry 4] In formula (2), R 1 It is an alkenyl group.
16. The dispersant for emulsion polymerization according to claim 15, in, In the formula (2), R 1 The alkenyl group shown has a methylene group at the terminal end on the carbonyl side.
17. The dispersant for emulsion polymerization according to any one of claims 13 to 16, in, The vinyl alcohol-based polymer has tertiary carbon atoms.
18. The dispersant for emulsion polymerization according to any one of claims 13 to 17, in, The vinyl alcohol polymer has a structural unit derived from an aliphatic unsaturated aldehyde.
19. The dispersant for emulsion polymerization according to claim 18, in, The aliphatic unsaturated aldehyde has 3 to 14 carbon atoms.
20. The dispersant for emulsion polymerization according to claim 18 or 19, in, The aliphatic unsaturated aldehyde has a carbon-carbon double bond at the terminal end.
21. The dispersant for emulsion polymerization according to any one of claims 13 to 20, in, The vinyl alcohol polymer has a saponification degree of 80 mol% or more. 22 . An aqueous emulsion comprising a polymer and the dispersant for emulsion polymerization according to claim 13 , wherein the polymer comprises a structural unit derived from at least one selected from an ethylenically unsaturated monomer and a diene monomer.
23. The aqueous emulsion according to claim 22, in, The ethylenically unsaturated monomer is at least one selected from styrene monomers, acrylate monomers and methacrylate monomers. 24 . A laminate comprising a substrate and a layer formed from the aqueous emulsion according to claim 22 or 23 .
25. The laminate according to claim 24, in, The substrate is paper. 26 . A laminate comprising a substrate and a layer containing the dispersant for emulsion polymerization according to claim 13 .
27. A method for producing an aqueous emulsion, wherein include: A step of emulsion-polymerizing at least one monomer selected from ethylenically unsaturated monomers and diene monomers in the presence of the dispersant for emulsion polymerization according to any one of claims 13 to 21.
28. The method for producing an aqueous emulsion according to claim 27, in, The ethylenically unsaturated monomer is at least one monomer selected from styrene monomers, acrylate monomers and methacrylate monomers.