Resin composition, prepreg, resin sheet, laminate, metal foil-clad laminate, and printed wiring board

By using a resin composition that covers the surface with titanium oxide and thermosetting compounds, combined with inorganic and organic oxide layer treatment, the problems of increased dielectric loss and interlayer delamination in printed circuit boards are solved, achieving high dielectric constant, low dielectric loss tangent, and excellent heat resistance and moisture absorption.

CN118974173APending Publication Date: 2024-11-15MITSUBISHI GAS CHEM CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028913.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-16
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In existing technologies for high-frequency printed circuit boards, increased dielectric loss leads to signal attenuation, and the filler material is prone to interlayer delamination, making it difficult to simultaneously achieve high dielectric constant, low dielectric loss tangent, and excellent heat resistance and moisture absorption.

Method used

A resin composition with a surface coating of titanium oxide and a thermosetting compound is used, wherein the surface coating of titanium oxide has a weight loss rate of less than 0.5% at a specific heating rate, and is combined with inorganic and organic oxide layer treatment, and the filler material includes silicon dioxide, etc., to form an insulating layer with high dielectric constant and low dielectric loss tangent.

Benefits of technology

It achieves high dielectric constant and low dielectric loss tangent, has excellent heat resistance and moisture-absorbing heat resistance, avoids interlayer delamination, and improves the reliability of printed circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005051307750000031
    Figure BDA0005051307750000031
  • Figure BDA0005051307750000041
    Figure BDA0005051307750000041
  • Figure BDA0005051307750000042
    Figure BDA0005051307750000042
Patent Text Reader

Abstract

The purpose of the present invention is to provide a resin composition, a prepreg obtained using the resin composition, a resin sheet, a laminate, a metal foil-clad laminate, and a printed wiring board. The resin composition is suitable for manufacturing an insulating layer of a printed circuit board having a high dielectric constant and a low dielectric loss tangent, and having excellent heat resistance and moisture absorption heat resistance. A resin composition according to the present invention contains: a surface-coated titanium oxide (A) having a weight loss ratio of 0.5 mass% or less when heated from 30 DEG C to 300 DEG C at a temperature increase rate of 10 DEG C / min; and a thermosetting compound (B).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, a prepreg, a resin sheet, a laminate, a metal foil-clad laminate and a printed circuit board. Background Art

[0002] In recent years, the signal frequency band of information communication equipment such as PHS and mobile phones and the CPU clock time (clock time) frequency of computers have reached the GHz band, and high frequency is in progress. The dielectric loss of electrical signals is proportional to the square root of the relative dielectric constant of the insulating layer forming the circuit, the dielectric loss tangent and the product of the frequency of the electrical signal. Therefore, the higher the frequency of the signal used, the greater the dielectric loss. The increase in dielectric loss can cause the electrical signal to attenuate and damage the reliability of the signal. Therefore, in order to suppress this situation, the insulating layer needs to select a material with a small dielectric constant and dielectric loss tangent.

[0003] On the other hand, the insulating layer of the high-frequency circuit has requirements such as the formation of a delay circuit, impedance integration of a wiring board in a low-impedance circuit, densification of a wiring pattern, and composite circuitization with a capacitor in the substrate itself, and sometimes requires a high dielectric constant of the insulating layer. Therefore, electronic parts (such as patent document 1) using an insulating layer with a high dielectric constant and a low dielectric loss tangent have been proposed. The insulating layer with a high dielectric constant and a low dielectric loss tangent is formed by dispersing filling materials such as ceramic powder and metal powder subjected to insulation treatment in a resin.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2000-91717 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] However, in order to increase the relative dielectric constant of the insulating layer, a filler having a high relative dielectric constant needs to be mixed, but at the same time, the dielectric loss tangent also increases, so there is a problem that the transmission loss of the high-frequency signal increases.

[0009] In addition, in the filling material used to manufacture the insulating layer with high dielectric constant and low dielectric loss tangent, gaps may be generated depending on the filling material mixed, causing interlayer delamination during the manufacture of the laminated board. Therefore, there is a problem of deterioration of dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance in printed circuit boards, etc.

[0010] In addition, if the insulating layer has low hygroscopic heat resistance, the moisture contained in the insulating layer will evaporate during reflow soldering to form voids, causing interlayer delamination during the manufacture of the laminate. Therefore, in the field of electronic materials that require high reliability, an insulating layer with excellent hygroscopic heat resistance is required.

[0011] The present invention is made to solve the above-mentioned problems, and its object is to provide a resin composition, a prepreg, a resin sheet, a laminate, a metal foil-clad laminate and a printed circuit board obtained by using the resin composition. The resin composition is suitable for use in manufacturing an insulating layer of a printed circuit board having a high dielectric constant and a low dielectric loss tangent and having excellent heat resistance and moisture absorption heat resistance.

[0012] Solutions for solving problems

[0013] The present inventors conducted intensive studies to solve the above-mentioned problems of the prior art and, as a result, found that a specific resin composition can solve the above-mentioned problems, thereby completing the present invention.

[0014] That is, the present invention is as follows.

[0015] [1] A resin composition comprising a surface-covered titanium oxide (A) and a thermosetting compound (B), wherein the surface-covered titanium oxide (A) has a weight loss rate of 0.5% by mass or less when heated from 30°C to 300°C at a heating rate of 10°C / min.

[0016] [2] The resin composition according to [1], wherein the surface-covering titanium oxide (A) has an organic layer and / or an inorganic oxide layer on the surface of titanium oxide particles.

[0017] [3] The resin composition according to [2], wherein the surface-covering titanium oxide (A) further has the organic layer on the surface of the inorganic oxide layer.

[0018] [4] The resin composition according to [2] or [3], wherein the total amount of the organic layer and the inorganic oxide layer is 0.1 to 10% by mass relative to 100% by mass of the surface-covering titanium oxide (A).

[0019] [5] The resin composition according to any one of [2] to [4], wherein the inorganic oxide layer is one or more selected from the group consisting of a layer containing silicon dioxide, a layer containing zirconium oxide, and a layer containing aluminum oxide.

[0020] [6] The resin composition according to any one of [2] to [5], wherein the organic layer is a layer surface-treated with an organic silicon compound.

[0021] [7] The resin composition according to [6], wherein the organosilicon compound includes one or more selected from the group consisting of a silane coupling agent, an organosilane, and an organopolysiloxane.

[0022] [8] The resin composition according to any one of [2] to [7], wherein the content of the titanium oxide in the surface-covering titanium oxide (A) is 90 to 99.9% by mass relative to 100% by mass of the surface-covering titanium oxide (A).

[0023] [9] The resin composition according to any one of [1] to [8], wherein the content of the surface-covering titanium oxide (A) is 50 to 500 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.

[0024]

[10] The resin composition according to any one of [1] to [9], wherein the thermosetting compound (B) comprises one or more selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, cyanate compounds, phenol compounds, alkenyl-substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having a polymerizable unsaturated group.

[0025]

[11] The resin composition according to

[10] , wherein the maleimide compound comprises one or more selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)-phenyl)propane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, a maleimide compound represented by the following formula (1), and a maleimide compound represented by the following formula (2).

[0026]

[0027] (In formula (1), R 1 Each independently represents a hydrogen atom or a methyl group, and n1 is an integer of 1 to 10. ).

[0028]

[0029] (In formula (2), R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, n2 is an average value, and 1 <n2≤5。)。

[0030]

[12] The resin composition according to

[10] or

[11] , wherein the epoxy compound comprises one or more selected from the group consisting of biphenyl aralkyl epoxy resins, naphthalene epoxy resins, and naphthyl ether epoxy resins.

[0031]

[13] The resin composition according to any one of

[10] to

[12] , wherein the modified polyphenylene ether compound includes a compound represented by the following formula (3).

[0032]

[0033] (In formula (3), X represents an aromatic group, -(YO)m- represents a polyphenylene ether portion. R1, R2 and R3 each independently represent a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group. m represents an integer from 1 to 100, n represents an integer from 1 to 6, and q represents an integer from 1 to 4.)

[0034]

[14] The resin composition according to any one of

[10] to

[13] , wherein the cyanate ester compound comprises one or more selected from the group consisting of phenol novolac type cyanate ester compounds, naphthol aralkyl type cyanate ester compounds, naphthyl ether type cyanate ester compounds, xylene resin type cyanate ester compounds, bisphenol M type cyanate ester compounds, bisphenol A type cyanate ester compounds, diallyl bisphenol A type cyanate ester compounds, bisphenol E type cyanate ester compounds, bisphenol F type cyanate ester compounds, biphenyl aralkyl type cyanate ester compounds, and prepolymers or polymers of these cyanate ester compounds.

[0035]

[15] The resin composition according to any one of [1] to

[14] , further comprising a filler (C) different from the surface-coating titanium oxide (A).

[0036]

[16] The resin composition according to

[15] , wherein the filler (C) comprises one or more selected from the group consisting of silica, alumina, barium titanate, strontium titanate, calcium titanate, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and silicone composite powder.

[0037]

[17] The resin composition according to

[15] or

[16] , wherein the content of the filler (C) is 50 to 300 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.

[0038]

[18] The resin composition according to any one of [1] to

[17] , which is used for a printed wiring board.

[0039]

[19] A prepreg comprising: a substrate, and the resin composition according to any one of [1] to

[18] impregnated or coated on the substrate.

[0040]

[20] A resin sheet comprising the resin composition according to any one of [1] to

[18] .

[0041]

[21] A laminate comprising one or more selected from the group consisting of the prepreg described in

[19] and the resin sheet described in

[20] .

[0042]

[22] A metal foil-clad laminate comprising: the laminate according to

[21] , and a metal foil disposed on one or both surfaces of the laminate.

[0043]

[23] A printed wiring board comprising: an insulating layer and a conductor layer disposed on one or both surfaces of the insulating layer, wherein the insulating layer comprises a cured product of the resin composition according to any one of [1] to

[18] .

[0044] Effects of the Invention

[0045] According to the resin composition of the present invention, a resin composition, a prepreg obtained using the resin composition, a resin sheet, a laminate, a metal foil-clad laminate, and a printed circuit board can be provided. The resin composition is suitable for use in manufacturing an insulating layer of a printed circuit board having a high dielectric constant and a low dielectric loss tangent and having excellent heat resistance and moisture absorption heat resistance. DETAILED DESCRIPTION

[0046] Hereinafter, a method for implementing the present invention (hereinafter referred to as "this embodiment") is described in detail. The following this embodiment is an example for illustrating the present invention and is not intended to limit the present invention to the following content. The present invention can be implemented by appropriately modifying it within the scope of its gist.

[0047] In the present embodiment, unless otherwise specified, "resin solid content" or "resin solid content in the resin composition" refers to the resin content excluding the surface-coated titanium oxide (A), filler (C), additives (silane coupling agent, wetting dispersant, curing accelerator and other components), and solvent (solvent) in the resin composition. "Total 100 parts by mass of resin solid content" or "total 100 parts by mass of resin solid content in the resin composition" means that the total of the resin content excluding the surface-coated titanium oxide (A), filler (C), additives (silane coupling agent, wetting dispersant, curing accelerator and other components), and solvent (solvent) in the resin composition is 100 parts by mass.

[0048] [Resin composition]

[0049] The resin composition of the present embodiment contains a surface-covered titanium oxide (A) and a thermosetting compound (B), wherein the surface-covered titanium oxide (A) has a weight loss rate of 0.5 mass % or less when heated from 30° C. to 300° C. at a temperature increase rate of 10° C. / min.

[0050] According to the present embodiment, it is possible to provide a cured product with high dielectric constant and low dielectric loss tangent and with excellent heat resistance (solder heat resistance) and hygroscopic heat resistance. That is, by using the resin combination of the present embodiment, it is possible to suitably manufacture a prepreg, resin sheet, plywood, metal foil-covered plywood and printed circuit board with high dielectric constant and low dielectric loss tangent and excellent heat resistance and hygroscopic heat resistance during solidification, it is possible to more suitably manufacture the insulating layer of a printed circuit board. Therefore, the resin combination of the present embodiment can be more suitably used to manufacture the insulating layer of a printed circuit board.

[0051] Particularly, the inventors have found that, by using a resin composition containing surface-covered titanium oxide (A) and a thermosetting resin (B) in the insulating layer of a printed circuit board, and the weight loss rate of the surface-covered titanium oxide (A) when heated from 30°C to 300°C at a heating rate of 10°C / minute is 0.5% by mass or less, it is not easy to produce gaps during reflow soldering, and it is not easy to cause interlayer peeling during the manufacture of laminated boards. Therefore, according to the present embodiment, due to having excellent adhesion in the insulating layer and the conductor layer, it is possible to obtain a printed circuit board with good heat resistance and hygroscopic heat resistance and good dielectric properties (high dielectric constant and low dielectric loss tangent). Its reason is not clear, but the inventors have speculated as follows. That is, usually, the surface-covered titanium oxide has a surface coating layer, so it is easier to absorb moisture in the atmosphere. In this case, in the cured product obtained using the surface-covered titanium oxide, the absorbed moisture will evaporate during reflow soldering, and a gap will be generated in the insulating layer. This situation will occur significantly when the surface-covered titanium oxide has an inorganic oxide layer as a surface coating layer. And, when the surface-covered titanium oxide has an organic layer as a surface covering layer, the organic component will decompose due to heat during reflow soldering, so the organic component volatilizes and is more likely to produce gaps. When the surface-covered titanium oxide has an inorganic oxide layer and an organic layer, both the evaporation of water and the volatilization of organic components will occur. However, if the weight loss rate when heated from 30°C to 300°C at a heating rate of 10°C / minute is less than 0.5% by mass, the evaporation of water and the volatilization of organic components can be appropriately suppressed. By using such a surface-covered titanium oxide (A) and a thermosetting resin (B) together, it is possible to have a high dielectric constant and a low dielectric loss tangent, and have excellent heat resistance and hygroscopic heat resistance, while the evaporation of water when having an inorganic oxide layer and the volatilization of organic components when having an organic layer can be appropriately suppressed. Therefore, the inventors speculate that according to the present embodiment, it is not easy to produce gaps during reflow soldering, and it is not easy to cause interlayer peeling during the manufacture of laminated boards. But the reason is not limited to this.

[0052] <Surface coating with titanium oxide (A)>

[0053] The resin composition of the present embodiment contains a surface-covered titanium oxide (A) having a weight loss rate of 0.5 mass % or less when heated from 30° C. to 300° C. at a temperature increase rate of 10° C. / min.

[0054] From the viewpoint of obtaining a resin composition having a higher dielectric constant and a lower dielectric loss tangent and having better heat resistance and hygroscopic heat resistance, the weight loss rate when heated from 30°C to 300°C at a heating rate of 10°C / min is preferably 0.48% by mass or less, more preferably 0.45% by mass or less, and further preferably 0.43% by mass. In addition, the lower limit is not particularly limited, for example, 0% or more. The method for determining the weight loss rate can be determined, for example, by thermogravimetric determination (TG), and the specific determination method is described in the examples.

[0055] The surface-coated titanium oxide (A) preferably has an organic layer and / or an inorganic oxide layer on the surface of the titanium oxide particles (hereinafter referred to as "titanium oxide particles" or "core particles") that serve as the core of the surface-coated titanium oxide (A). The surface-coated titanium oxide (A) may be used alone or in combination of two or more surface-coated titanium oxides having different particle sizes and surface states.

[0056] From the viewpoint of dispersibility, the average particle size (D50) of the surface-covered titanium oxide (A) is preferably 0.1 to 5 μm, and more preferably 0.15 to 1 μm. It should be noted that in this specification, the average particle size (D50) refers to the value obtained by measuring the particle size distribution of a powder added to a dispersion medium in a specified amount using a laser diffraction-scattering particle size distribution measuring device, and accumulating the volume from small particles until it reaches 50% of the total volume. The average particle size (D50) can be obtained by measuring the particle size distribution using a laser diffraction-scattering method, and the specific measurement method can be referred to the examples.

[0057] The shape of the surface-coated titanium oxide (A) is not particularly limited, and examples thereof include flaky, spherical, plate-like, and irregular shapes. The shape is preferably spherical from the viewpoint of having good dispersibility with the thermosetting compound (B) described later, obtaining a resin composition having better heat resistance and moisture absorption heat resistance during curing, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent), and further obtaining an insulating layer having a more suitable surface hardness.

[0058] The relative dielectric constant of the surface-coated titanium oxide (A) is preferably more than 20, more preferably more than 25. If the relative dielectric constant is more than 20, there is a tendency to obtain an insulating layer with a high relative dielectric constant. It should be noted that the relative dielectric constant of the surface-coated titanium oxide (A) in the present embodiment is a value at 10 GHz measured using a cavity resonator vibration method. In the present embodiment, the relative dielectric constant of the surface-coated titanium oxide (A) can be obtained using the Bruggeman formula (composite rule).

[0059] The dielectric loss tangent of the surface-coated titanium oxide (A) is preferably less than 0.01, more preferably less than 0.008. If the dielectric loss tangent is less than 0.01, there is a tendency to obtain an insulating layer with low dielectric loss tangent. It should be noted that, in the present embodiment, the dielectric loss tangent of the surface-coated titanium oxide (A) is the value at 10 GHz measured using a cavity resonator method. In the present embodiment, the dielectric loss tangent of the surface-coated titanium oxide (A) can be obtained using Bruggeman's formula (composite rule).

[0060] From the viewpoints of obtaining a printed wiring board having better heat resistance and moisture absorption heat resistance and good dielectric properties (high dielectric constant and low dielectric loss tangent), further improving adhesion with the resin component, further alleviating aggregation of the surface-covering titanium oxide (A) in the resin composition, further improving dispersibility, and obtaining excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance, the total amount (covering amount) of the organic layer and the inorganic oxide layer in the surface-covering titanium oxide (A) is preferably 0.1 to 10% by mass, more preferably 1 to 8% by mass, and even more preferably 1 to 4% by mass relative to 100% by mass of the surface-covering titanium oxide (A).

[0061] From the viewpoint of obtaining a printed circuit board having better heat resistance and moisture absorption heat resistance, and good dielectric properties (high dielectric constant and low dielectric loss tangent), further improving the adhesion with the resin component, further alleviating the aggregation of the surface-covering titanium oxide (A) in the resin composition, further improving the dispersibility, and obtaining excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance, the content of titanium oxide in the surface-covering titanium oxide (A) is preferably 90 to 99.9% by mass, more preferably 92 to 99% by mass, and further preferably 96 to 99% by mass relative to 100% by mass of the surface-covering titanium oxide (A).

[0062] Examples of the core particles include titanium monoxide (TiO), titanium trioxide (Ti2O3), and titanium dioxide (TiO2). Titanium dioxide is preferred among these. Titanium dioxide preferably has a rutile or anatase crystal structure, and more preferably has a rutile crystal structure.

[0063] From the viewpoint of dispersibility, the average particle size (D50) of the core particles is preferably 0.10 to 0.45 μm, and more preferably 0.15 to 0.25 μm. In the present embodiment, the average particle size (D50) of the core particles is obtained from the average value of the particle sizes of primary particles based on a single particle.

[0064] Surface-coated titanium oxide (A) can be obtained by using a surface treatment agent to cover an organic layer or an inorganic oxide layer on the surface of the core particle. In addition, on the surface of the organic layer or inorganic oxide layer covering the surface of the core particle, it is also possible to use a surface treatment agent to further cover the organic layer and / or the inorganic oxide layer. For the printed circuit board with better heat resistance and hygroscopic heat resistance and good dielectric properties (high dielectric constant and low dielectric loss tangent) etc., more improved adhesion with resin components, more relaxed surface-coated titanium oxide (A) in the resin composition Aggregation, more improved dispersibility, can obtain excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent heat resistance and hygroscopic heat resistance The viewpoint of the cured product, surface-coated titanium oxide (A) preferably has an organic layer on the surface of the inorganic oxide layer covering the surface of the core particle. As a covering method, inorganic treatment and organic treatment can be cited. Surface treatment agent can be used alone 1, or two or more can be used in combination.

[0065] As the surface treatment agent used for inorganic treatment, for example, oxygen-containing acids (such as silicic acid and aluminic acid) of metals such as aluminum, silicon, zirconium, tin, titanium, antimony, zinc, cobalt and manganese, metal salts of oxygen-containing acids (such as sodium silicate and sodium aluminate), oxides, hydroxides and hydrated oxides, etc. The surface-covered titanium oxide (A) obtained by inorganic treatment has an inorganic oxide layer on the surface of the titanium oxide particles, the surface of the inorganic oxide layer, or the surface of the organic layer described later.

[0066] As the surface treatment agent used for organic treatment, for example, organic silicon compounds such as organic silane, silane coupling agent and organic polysiloxane; organic titanium compounds such as titanium coupling agent; organic substances such as organic acid, polyol and alkanolamine, etc. The surface-coated titanium oxide (A) obtained by organic treatment has an organic layer on the surface of titanium oxide particles, the surface of the organic layer, or the surface of the inorganic oxide layer.

[0067] Examples of the organosilane include alkoxysilanes such as n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, 3-chloropropyltriethoxysilane, phenyltriethoxysilane and trifluoropropyltrimethoxysilane.

[0068] Examples of the silane coupling agent include aminosilanes such as 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane; epoxysilanes such as 3-glycidoxypropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; methacrylic silanes such as 3-(methacryloxypropyl)trimethoxysilane; vinylsilanes such as vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltrichlorosilane; and mercaptosilanes such as 3-mercaptopropyltrimethoxysilane.

[0069] As the organopolysiloxane, silicone oil is preferred because a more uniform organic layer can be formed. Examples of the silicone oil include alkyl silicone, alkyl hydrogen silicone, alkoxy silicone, and modified silicone.

[0070] As an example of alkyl silicone, dimethyl silicone can be mentioned.

[0071] Examples of the alkyl hydrogen silicone include methyl hydrogen silicone and ethyl hydrogen silicone.

[0072] As alkoxy silicone, preferably, a silicone compound containing an alkoxysilyl group formed by an alkoxy group directly bonded to a silicon atom or bonded via a divalent hydrocarbon group. As such silicone compound, for example, linear, cyclic, network, and partially branched linear organopolysiloxanes can be cited. Among them, linear organopolysiloxanes are preferred, and organopolysiloxanes having a molecular structure in which an alkoxy group is directly bonded to a silicone main chain are more preferred. As alkoxy silicone, for example, methoxy silicone and ethoxy silicone can be cited.

[0073] Examples of the modified silicone include amino-modified silicone, epoxy-modified silicone, and mercapto-modified silicone.

[0074] Examples of the titanium coupling agent include isopropyl triisostearoyl titanate, isopropyl dimethacryloyl isostearyl titanate, and isopropyl tridodecylbenzenesulfonyl titanate.

[0075] Examples of the organic acid include adipic acid, terephthalic acid, lauric acid, myristic acid, palmitic acid, stearic acid, polyhydroxystearic acid, oleic acid, salicylic acid, malic acid, maleic acid, and metal salts thereof.

[0076] Examples of the polyol include trimethylolethane, trimethylolpropane, di(trimethylol)propane, ethoxylated trimethylolpropane, and pentaerythritol.

[0077] Examples of the alkanolamine include monoethanolamine, monopropanolamine, diethanolamine, dipropanolamine, triethanolamine, and tripropanolamine.

[0078] From the viewpoint of having good dispersibility with the thermosetting compound (B), obtaining a resin composition having better heat resistance and moisture absorption heat resistance and better dielectric properties (high dielectric constant and low dielectric loss tangent) when cured, and further obtaining an insulating layer with more suitable surface hardness, the surface-coated titanium oxide (A) preferably has an inorganic oxide layer on the surface of the titanium oxide particles, and the inorganic oxide layer is one or more selected from the group consisting of a layer containing silicon dioxide, a layer containing zirconium oxide, and a layer containing aluminum oxide. More preferably, the inorganic oxide layer is one or more selected from the group consisting of a layer containing silicon dioxide and a layer containing aluminum oxide.

[0079] The surface-coated titanium oxide (A) may also have two or more inorganic oxide layers. When having two or more inorganic oxide layers, it is preferably configured as follows: the inorganic oxide layer located near the titanium oxide particle side can mainly further suppress the water absorption caused by the core particle, i.e., the titanium oxide particle, and the inorganic oxide layer located far from the titanium oxide particle side can mainly improve the adhesion with the resin component, the aggregation relaxation of the surface-coated titanium oxide (A) in the resin composition, and the dispersibility.

[0080] From this viewpoint, when the surface-covered titanium oxide (A) has two or more inorganic oxide layers, it is preferred that the inorganic oxide layer located on the side close to the core particle is one or more selected from the group consisting of a layer containing silicon dioxide and a layer containing zirconium oxide, and the inorganic oxide layer located on the side away from the core particle is a layer containing aluminum oxide, and it is more preferred that the inorganic oxide layer located on the side close to the core particle is a layer containing silicon dioxide, and the inorganic oxide layer located on the side away from the core particle is a layer containing aluminum oxide.

[0081] From the viewpoint of obtaining a printed circuit board having better heat resistance and moisture absorption heat resistance, and better dielectric properties (high dielectric constant and low dielectric loss tangent), and excellent heat resistance of the cured product, the total amount of the inorganic oxide layer is preferably 0.1 to 10 mass %, more preferably 0.3 to 7.5 mass %, further preferably 0.4 to 5.0 mass %, further preferably 0.5 to 4.0 mass %, and further preferably 0.5 to 3.3 mass %, relative to 100 mass % of the surface-covered titanium oxide (A).

[0082] The inorganic oxide layer has the effect of suppressing the water absorption caused by the core particle, i.e., titanium oxide. On the other hand, silicon dioxide, zirconium oxide, and aluminum oxide, which are inorganic oxides constituting the inorganic oxide layer, are hydrated inorganic substances, and therefore have a tendency to have a higher water absorption rate among inorganic oxides and to easily evaporate water in reflow soldering. The evaporated water can become the cause of the generation of voids in the insulating layer. From such a viewpoint, the surface-coated titanium oxide (A) preferably has an organic layer on the surface of the inorganic oxide layer. The organic layer can further reduce the water absorption of the core particle, i.e., titanium oxide, and the inorganic oxide layer, and further suppress the water absorption of the resin composition. Therefore, in reflow soldering, the evaporation of water from the insulating layer can be suppressed. In addition, the organic layer can also play an effect of making the aggregation of the surface-coated titanium oxide (A) in the resin composition more moderate and improving the dispersibility.

[0083] The organic layer is preferably a layer surface-treated with an organosilicon compound from the viewpoint of further alleviating aggregation of the surface-coating titanium oxide (A) in the resin composition, further improving dispersibility, and reducing the water absorption of the laminate due to better water repellency.

[0084] As the organosilicon compound, it is preferred to include more than one selected from the group consisting of a silane coupling agent, an organosilane, and an organopolysiloxane. By using these surface treatment agents to carry out surface treatment, the obtained organic layer becomes a layer with a siloxane structure. The layer with a siloxane structure has a tendency to further alleviate the aggregation of the surface-covered titanium oxide (A) in the resin composition, further improve dispersibility, and reduce the water absorption rate of the laminate due to more excellent water repellency. In addition, from the viewpoint that a layer with a more uniform siloxane structure can be formed and the above-mentioned effect can be further exerted, the organopolysiloxane is preferably silicone oil, and among the silicone oil, dimethyl silicone is more preferably used. In addition, if the organic layer becomes a layer with a siloxane structure, a surface treatment agent other than the above-mentioned can also be used.

[0085] From the viewpoint of further alleviating the aggregation of the surface-covering titanium oxide (A) in the resin composition and further improving the dispersibility, the total amount of the organic layer is preferably 0.1 to 10% by mass, more preferably 0.5 to 7.5% by mass, further preferably 0.6 to 6.0% by mass, further preferably 0.7 to 5.0% by mass, and further preferably 0.7 to 3.5% by mass, relative to 100% by mass of the surface-covering titanium oxide (A).

[0086] When the surface-coated titanium oxide (A) has an inorganic oxide layer and an organic layer, the covering layer of the surface-coated titanium oxide (A) can also be a 2-layer structure of an inorganic oxide layer and an organic layer. By setting it to such a layer structure, the catalytic activity (such as photocatalytic activity and metal catalytic activity) of titanium oxide can be exerted and the effect of water repellency. At this time, the inorganic oxide layer is preferably selected from the group consisting of a layer comprising silicon dioxide, a layer comprising zirconium oxide, and a layer comprising aluminum oxide. More than one, for the purpose of further improving the affinity with the resin and further suppressing the catalytic activity of titanium oxide, more preferably a layer comprising aluminum oxide. From the viewpoint of excellent heat resistance and chemical stability, the organic layer preferably has a siloxane structure. By using such a surface-covered titanium oxide (A), the water absorption of the titanium oxide can be further suppressed, and the adhesion with the resin component can be further improved. The aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, and the dispersibility with the thermosetting compound (B) is further improved. A resin composition having further excellent heat resistance and moisture absorption heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) during curing can be obtained, and an insulating layer having a more suitable surface hardness can be obtained.

[0087] As such a surface-coated titanium oxide (A), a commercially available product can be used. Examples of the commercially available product include R-22L and R-11P (these are trade names, SAKAI CHEMICAL INDUSTRY CO., LTD.).

[0088] When the surface-covered titanium oxide (A) has an inorganic oxide layer and an organic layer, it is preferred that the inorganic oxide layer located near the core particle side is a layer comprising silicon dioxide, and then the inorganic oxide layer is a layer comprising aluminum oxide, and the organic layer located at the farthest side from the core particle is a layer having a siloxane structure. By using such a surface-covered titanium oxide (A), the water absorption of titanium oxide can be further suppressed, and the adhesion with the resin component can be further improved, and the aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, and it has a further good dispersibility with the thermosetting compound (B), and a resin composition having further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when curing, and then an insulating layer with further suitable surface hardness can be obtained.

[0089] As such a surface-coating titanium oxide (A), a commercially available product can be used. Examples of the commercially available product include CR-63 (trade name, ISHIHARA SANGYO KAISHA, LTD.).

[0090] The content of the surface-coated titanium oxide (A) is preferably 50 to 500 parts by mass, more preferably 60 to 450 parts by mass, and further preferably 70 to 400 parts by mass relative to a total of 100 parts by mass of the resin solid component in the resin composition. By making the content of the surface-coated titanium oxide (A) within the above range, there is a tendency to obtain a resin composition having further good dispersibility with the thermosetting compound (B), further excellent heat resistance and hygroscopic heat resistance, and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent), and further to obtain an insulating layer having a further suitable surface hardness.

[0091] <Thermosetting Compound (B)>

[0092] The resin composition of the present embodiment contains a thermosetting compound (B).

[0093] The thermosetting compound (B) is not particularly limited as long as it is a thermosetting compound or resin. The thermosetting compound (B) may be used alone or in combination of two or more.

[0094] From the viewpoint that the surface-covered titanium oxide (A) is further well dispersed, and a resin composition having further excellent heat resistance and hygroscopic heat resistance and more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when cured, the thermosetting compound (B) preferably includes one or more thermosetting compounds or resins (hereinafter also referred to as "thermosetting resins") selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, cyanate compounds, phenol compounds, alkenyl-substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having polymerizable unsaturated groups. These thermosetting resins can be used alone or in combination of two or more.

[0095] From the viewpoint that the surface-coated titanium oxide (A) is further well dispersed and a resin composition having further excellent heat resistance and moisture absorption heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when cured, the thermosetting compound (B) is more preferably one or more selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, cyanate compounds, phenol compounds, and compounds having a polymerizable unsaturated group, and is further preferably one or more selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, and cyanate compounds.

[0096] Surface-coated titanium oxide (A) can suitably suppress the electrophilicity of Lewis acidity produced by titanium oxide by carrying out surface coating. Therefore, in resin combination, even if surface-coated titanium oxide (A) and thermosetting compound (B) are close, the polymerization of thermosetting compound (B) will not be carried out intentionally, and poor curing, viscosity rise, etc. can be prevented. In addition, surface-coated titanium oxide (A) can also suitably suppress the hydrolysis for thermosetting compound (B) by carrying out surface coating, so the amount of unreacted functional groups in insulating layer can be reduced. Therefore, according to the resin combination of the present embodiment, the amount of moisture contained in insulating layer during reflow can be suitably suppressed, so it is not easy to produce voids, and when the manufacture of laminated board, it is not easy to cause interlayer peeling. From the viewpoint of further suppressing the progress of polymerization and hydrolysis, thereby obtaining a resin composition having further excellent heat resistance and hygroscopic heat resistance as well as further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) during curing, the thermosetting compound (B) further preferably contains one or more selected from the group consisting of maleimide compounds and cyanate ester compounds.

[0097] From the viewpoint of obtaining a resin composition having further excellent heat resistance and moisture absorption heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when curing by further dispersing the surface-coated titanium oxide (A) and the thermosetting compound (B) in a mass ratio (surface-coated titanium oxide (A): thermosetting compound (B)), the surface-coated titanium oxide (A) and the thermosetting compound (B) are preferably 30:70 to 90:10, more preferably 35:65 to 85:15, and even more preferably 40:60 to 80:20.

[0098] (Maleimide compound)

[0099] For surface-covered titanium oxide (A) further well dispersed, can obtain when solidifying, have further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) resin composition viewpoint, the resin composition of the present embodiment preferably includes maleimide compound.In addition, for obtaining significantly based on surface-covered titanium oxide (A), suppressing polymerization and the effect of hydrolysis, also preferably maleimide compound.And then, if resin composition contains maleimide compound, then have and surface-covered titanium oxide (A) adhesion more improve, can more relax the aggregation of the surface-covered titanium oxide (A) in resin composition, more improve dispersibility, can obtain excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and the tendency of heat resistance.

[0100] If the maleimide compound is a compound having one or more maleimide groups in one molecule, a known one can be used appropriately, and its type is not particularly limited. The number of maleimide groups in one molecule of the maleimide compound is 1 or more, preferably 2 or more. The maleimide compound can be used alone or in combination of two or more.

[0101] Examples of the maleimide compound include N-phenylmaleimide, N-hydroxyphenylmaleimide, bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane, bis(3,5-dimethyl-4-maleimidephenyl)methane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, bis(3,5-diethyl-4-maleimidephenyl)methane, the maleimide compound represented by formula (1), the maleimide compound represented by formula (2), prepolymers of these maleimide compounds, and prepolymers of the above maleimide compounds and amine compounds.

[0102] Among them, the maleimide compound preferably contains one or more selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, the maleimide compound represented by formula (1) and the maleimide compound represented by formula (2), and more preferably contains one or more selected from the group consisting of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane and the maleimide compound represented by formula (2), from the viewpoint that the surface-coated titanium oxide (A) is further well dispersed, a resin composition having further excellent heat resistance and moisture absorption heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when cured, and an insulating layer having suitable surface hardness can be obtained. Furthermore, when the resin composition contains these maleimide compounds, there is a tendency that the adhesion with the surface-coated titanium oxide (A) is further improved, the aggregation of the surface-coated titanium oxide (A) in the resin composition can be further alleviated, the dispersibility can be further improved, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance can be obtained.

[0103]

[0104] In formula (1), R 1 Each independently represents a hydrogen atom or a methyl group, and n1 is an integer of 1-10.

[0105]

[0106] In formula (2), R 2Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, n2 is an average value, and 1 <n2≤5。

[0107] Relative to a total of 100 parts by mass of the resin solids in the resin composition, the content of the maleimide compound is preferably 10 to 85 parts by mass, more preferably 15 to 80 parts by mass, further preferably 20 to 75 parts by mass, further preferably 25 to 70 parts by mass, and further preferably 20 to 60 parts by mass. By making the content of the maleimide compound within the above range, there is a tendency that the surface-covered titanium oxide (A) is further well dispersed, a resin composition having further excellent heat resistance and hygroscopic heat resistance and more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when curing, and then an insulating layer with further suitable surface hardness can be obtained. Furthermore, by making the content of the maleimide compound within the above range, there is a tendency that the adhesion with the surface-covered titanium oxide (A) is further improved, the aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, the dispersibility is further improved, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance can be obtained.

[0108] Commercially available maleimide compounds may be used, or products manufactured by a known method may be used. Commercially available maleimide compounds include, for example, BMI-70, BMI-80, and BMI-1000P (the above are trade names, K.I. Chemical Industry Co., LTD.); BMI-3000, BMI-4000, BMI-5100, BMI-7000, and BMI-2300 (maleimide compounds represented by the above formula (1), wherein R 1 All are hydrogen atoms, and n1 is an integer of 1 to 5) (the above are trade names, Daiwa Fine Chemicals Co., Ltd.); MIR-3000-70MT (trade name, the maleimide compound represented by the above formula (2), in which R 2 All are hydrogen atoms, n2 is an average value, and 1<n2≤5. Nippon Kayaku Co., Ltd.) etc.

[0109] (Epoxides)

[0110] For the surface-covered titanium oxide (A) further well dispersed, can obtain when solidifying, have further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) resin composition viewpoint, the resin composition of the present embodiment preferably contains epoxy compound.In addition, if resin composition contains epoxy compound, then have with the surface-covered titanium oxide (A) adhesion more improved, can further relax the aggregation of the surface-covered titanium oxide (A) in the resin composition, further improve dispersibility, can obtain excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and the tendency of heat resistance.

[0111] If the epoxy compound is a compound having one or more epoxy groups in one molecule, a known epoxy compound may be used appropriately, and its type is not particularly limited. The number of epoxy groups per one molecule of the epoxy compound is 1 or more, preferably 2 or more. The epoxy compound may be used alone or in combination of two or more.

[0112] As the epoxy compound, conventionally known epoxy compounds and epoxy resins can be used. For example, biphenyl aralkyl epoxy resins, naphthalene epoxy resins, binaphthyl epoxy resins, multifunctional phenol epoxy resins, naphthyl ether epoxy resins, phenol aralkyl epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, xylene novolac epoxy resins, naphthalene skeleton modified novolac epoxy resins, dicyclopentadiene novolac epoxy resins, biphenyl novolac epoxy resins, phenol aralkyl novolac epoxy resins, naphthol aralkyl novolac epoxy resins, aralkyl novolac epoxy resins, aromatic hydrocarbon formaldehyde epoxy compounds, anthraquinone epoxy compounds, anthracene epoxy resins, naphthol aralkyl cyclo Oxygen compounds, dicyclopentadiene type epoxy resins, xylok type epoxy compounds, bisphenol A type epoxy resins, bisphenol E type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol A novolac type epoxy resins, phenol type epoxy compounds, biphenyl type epoxy resins, aralkyl novolac type epoxy resins, triazine skeleton epoxy compounds, triglycidyl isocyanurate, alicyclic epoxy resins, polyol type epoxy resins, glycidyl amine, glycidyl ester resins, compounds obtained by epoxidizing double bonds of double bond-containing compounds such as butadiene, and compounds obtained by reacting hydroxyl-containing silicone resins with epichlorohydrin, etc.

[0113] Among them, for making the surface-covered titanium oxide (A) further well dispersed, it is possible to obtain the viewpoint of the resin composition having further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when solidified, the epoxy compound preferably includes more than one selected from the group consisting of biphenyl aralkyl epoxy resin, naphthalene type epoxy resin and naphthyl ether type epoxy resin, more preferably naphthalene type epoxy resin. And then, if the resin composition contains these epoxy resins, there is a tendency to further improve the adhesion with the surface-covered titanium oxide (A), further alleviate the aggregation of the surface-covered titanium oxide (A) in the resin composition, further improve dispersibility, obtain excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance.

[0114] As the naphthalene type epoxy resin, commercially available products may be used, and examples thereof include EPICLON (registered trademark) EXA-4032-70M and EPICLON (registered trademark) HP-4710 (these are trade names, manufactured by DIC Corporation).

[0115] Relative to a total of 100 parts by mass of the resin solids in the resin composition, the content of the epoxy compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and further preferably 10 to 30 parts by mass. By making the content of the epoxy compound within the above range, there is a tendency to be more excellent in adhesion and flexibility. By making the content of the epoxy resin within the above range, there is a tendency that the surface-covered titanium oxide (A) is further well dispersed, a resin composition having further excellent heat resistance and hygroscopic heat resistance and more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when curing, and then an insulating layer with further suitable surface hardness can be obtained. In addition, there is a tendency that the adhesion with the surface-covered titanium oxide (A) is further improved, the aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, the dispersibility is further improved, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance can be obtained.

[0116] (Modified polyphenylene ether compound)

[0117] For surface-covered titanium oxide (A) further well dispersed, can obtain when solidifying, have further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) resin composition viewpoint, the resin composition of the present embodiment preferably comprises modified polyphenylene ether compound.In addition, if resin composition contains modified polyphenylene ether compound, then have with surface-covered titanium oxide (A) close adhesion more improved, can more relax the aggregation of surface-covered titanium oxide (A) in resin composition, more improve dispersibility, can obtain excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and the tendency of heat resistance.

[0118] In this specification, the "modification" of the modified polyphenylene ether compound means that part or all of the terminal of the polyphenylene ether compound is substituted with a reactive functional group such as a carbon-carbon unsaturated double bond. If part or all of the terminal of the polyphenylene ether compound in the modified polyphenylene ether compound is modified, a known one can be used appropriately without particular limitation. The modified polyphenylene ether compound can be used alone or in combination of two or more.

[0119] Examples of the polyphenylene ether compound as the modified polyphenylene ether compound include polymers containing at least one structural unit selected from the group consisting of the structural unit represented by formula (4), the structural unit represented by formula (5), and the structural unit represented by formula (6).

[0120]

[0121] In formula (4), R8, R9, R 10 and R 11 Each independently represents an alkyl group having 6 or less carbon atoms, an aryl group, a halogen atom or a hydrogen atom.

[0122]

[0123] In formula (5), R 12 , R 13 , R 14 , R 18 , R 19 Each independently represents an alkyl group having 6 or less carbon atoms or a phenyl group. 15 , R 16 , R 17 Each independently represents a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group.

[0124]

[0125] In formula (6), R 20 , R 21 , R 22 , R 23 , R 24 , R25 , R 26 , R 27 Each independently represents a hydrogen atom, an alkyl group having no greater than 6 carbon atoms, or a phenyl group. -A- is a linear, branched, or cyclic divalent hydrocarbon group having no greater than 20 carbon atoms.

[0126] Examples of -A- in formula (6) include, but are not limited to, divalent organic groups such as methylene, ethylidine, 1-methylethylidene, 1,1-propylidene, 1,4-phenylenebis(1-methylethylidene), 1,3-phenylenebis(1-methylethylidene), cyclohexylidene, phenylmethylene, naphthylmethylene, and 1-phenylethylidene.

[0127] Preferred modified polyphenylene ether compounds include, for example, those having ethylenically unsaturated groups such as vinylbenzyl groups, epoxy groups, amino groups, hydroxyl groups, mercapto groups, carboxyl groups, methacryl groups, and silyl groups at some or all of the ends of the polyphenylene ether compounds.

[0128] Examples of the modified polyphenylene ether compound having a hydroxyl group at the end include SA90 (trade name, SABIC Innovative Plastics Co., Ltd.) and the like.

[0129] Examples of the polyphenylene ether having a methacryloyl group at the end include SA9000 (trade name, SABIC Innovative Plastics Co., Ltd.) and the like.

[0130] The method for producing the modified polyphenylene ether compound is not particularly limited as long as the effects of the present invention can be obtained. For example, the modified polyphenylene ether compound can be produced by the method described in Japanese Patent No. 4591665.

[0131] The modified polyphenylene ether compound more preferably includes a modified polyphenylene ether compound having an ethylenically unsaturated group at the terminal. Examples of the ethylenically unsaturated group include alkenyl groups such as vinyl, allyl, acryloyl, methacryloyl, propenyl, butenyl, hexenyl, and octenyl; cycloalkenyl groups such as cyclopentenyl and cyclohexenyl; and alkenylaryl groups such as vinylbenzyl and vinylnaphthyl. Among them, vinylbenzyl is preferred.

[0132] The terminal ethylenically unsaturated groups may be single or multiple and may be the same functional groups or different functional groups.

[0133] From the viewpoint that the surface-covered titanium oxide (A) is further well dispersed, and a resin composition having further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when solidified, the modified polyphenylene ether compound having an ethylenically unsaturated group at the end is preferably a compound shown in formula (3). In addition, if the resin composition contains the compound shown in formula (3), there is a tendency that the adhesion with the surface-covered titanium oxide (A) is further improved, the aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, the dispersibility can be further improved, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance can be obtained.

[0134]

[0135] In formula (3), X represents an aromatic group, -(YO) m - represents a polyphenylene ether moiety. R1, R2, and R3 each independently represent a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, m represents an integer of 1 to 100, n represents an integer of 1 to 6, and q represents an integer of 1 to 4. m is preferably an integer of 1 to 50, and more preferably an integer of 1 to 30. In addition, n is preferably an integer of 1 to 4, and more preferably 1 or 2, and 1 is more ideal. In addition, q is preferably an integer of 1 to 3, and more preferably 1 or 2, and 2 is more ideal.

[0136] Examples of the aromatic group represented by X in formula (3) include groups obtained by removing q hydrogen atoms from one ring structure selected from a benzene ring structure, a biphenyl ring structure, an indene ring structure, and a naphthalene ring structure (e.g., phenylene, biphenylene, indenylene, and naphthylene). Among them, biphenylene is preferred.

[0137] Here, the aromatic group represented by X may include a diphenyl ether group in which an aryl group is bonded via an oxygen atom, a benzophenone group in which an aryl group is bonded via a carbonyl group, a 2,2-diphenylpropane group in which an aryl group is bonded via an alkylene group, and the like.

[0138] In addition, the aromatic group may be substituted with a common substituent such as an alkyl group (preferably an alkyl group having 1 to 6 carbon atoms, particularly a methyl group), an alkenyl group, an alkynyl group, a halogen atom, etc. However, since the aromatic group is substituted on the polyphenylene ether portion via an oxygen atom, the limit of the number of substituents generally depends on the number of polyphenylene ether portions.

[0139] As the polyphenylene ether portion in formula (3), the structural unit represented by formula (4), the structural unit represented by formula (5), and the structural unit represented by formula (6) can be used. Among them, it is more preferable to include the structural unit represented by formula (4).

[0140] In addition, as the modified polyphenylene ether compound represented by formula (3), the number average molecular weight is preferably 500 or more and 7000 or less. In addition, the one with the lowest melt viscosity of 50000 Pa·s or less in formula (3) can be used. From the viewpoint that the surface-coated titanium oxide (A) is further well dispersed and a resin composition having further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained during curing, the one with the number average molecular weight of 1000 or more and 7000 or less in formula (3) and the lowest melt viscosity of 50000 Pa·s or less is preferably obtained.

[0141] The number average molecular weight is measured using a gel permeation chromatograph according to a predetermined method. The number average molecular weight is more preferably 1,000 or more and 3,000 or less.

[0142] The minimum melt viscosity is measured using a dynamic viscoelasticity measuring apparatus according to a predetermined method. The minimum melt viscosity is more preferably 500 Pa·s or more and 50000 Pa·s or less.

[0143] As the modified polyphenylene ether compound, in the formula (3), a compound represented by the following formula (7) is preferred.

[0144]

[0145] In formula (7), X is an aromatic group, -(YO) m - each represents a polyphenylene ether moiety, and m represents an integer of 1 to 100. m is preferably an integer of 1 to 50, and more preferably an integer of 1 to 30.

[0146] In formula (7), X, -(YO) m -, and m have the same meanings as in formula (3).

[0147] Preferably, X in formula (3) and formula (7) is formula (8), formula (9) or formula (10), and -(YO) in formula (3) and formula (7) m -and-(OY) m - is a structure in which the formula (11) or the formula (12) is arranged, or a structure in which the formula (11) and the formula (12) are arranged in blocks or randomly.

[0148]

[0149] In formula (9), R 28 , R 29 , R 30 and R 31 Each independently represents a hydrogen atom or a methyl group. -B- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.

[0150] Specific examples of -B- include the same specific examples as those of -A- in formula (6).

[0151]

[0152] In the formula (10), -B- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.

[0153] Specific examples of -B- include the same specific examples as those of -A- in formula (6).

[0154]

[0155] The method for producing the modified polyphenylene ether compound having the structure represented by formula (7) is not particularly limited, and it can be produced, for example, by vinylbenzyl etherifying the terminal phenolic hydroxyl group of a bifunctional phenylene ether oligomer obtained by oxidative coupling of a bifunctional phenol compound and a monofunctional phenol compound.

[0156] In addition, such modified polyphenylene ether compounds can use commercially available products, for example, OPE-2St1200 (in formula (7), X in -(OXO)- is the structure represented by formula (8), and -(OY)- and -(YO)- are polymerized from the structure of formula (11)) and OPE-2st2200 (in formula (7), X in -(OXO)- is the structure represented by formula (8), and -(OY)- and -(YO)- are polymerized from the structure of formula (11)) (the above are trade names, Mitsubishi Gas Chemical Co., Ltd.) can be preferably used.

[0157] Relative to a total of 100 parts by mass of the resin solids in the resin composition, the content of the modified polyphenylene ether compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and further preferably 10 to 30 parts by mass. By making the content of the modified polyphenylene ether compound within the above range, there is a tendency for low dielectric loss tangent and reactivity to be further improved. By making the content of the modified polyphenylene ether compound within the above range, there is a tendency for the surface-coated titanium oxide (A) to be further well dispersed, a resin composition having further excellent heat resistance and hygroscopic heat resistance and more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) during curing to be obtained, and then an insulating layer having a further suitable surface hardness can be obtained. In addition, there is a tendency for the adhesion with the surface-coated titanium oxide (A) to be further improved, the aggregation of the surface-coated titanium oxide (A) in the resin composition to be further alleviated, the dispersibility to be further improved, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance to be obtained.

[0158] (Cyanate ester compound)

[0159] For surface-covered titanium oxide (A) further well dispersed, can obtain when solidifying, have further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) resin composition viewpoint, the resin composition of the present embodiment preferably includes cyanate ester compounds.In addition, for obtaining significantly based on surface-covered titanium oxide (A) suppressing polymerization to carry out and the effect of hydrolysis, cyanate ester compounds are also preferred.And then, if resin composition includes cyanate ester compounds, then there is the adhesion with surface-covered titanium oxide (A) more improved, can more relax the aggregation of the surface-covered titanium oxide (A) in the resin composition, more improve dispersibility, can obtain excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and the tendency of heat resistance.

[0160] As the cyanate compound, any known cyanate compound can be used as long as it has two or more cyano groups (also called "cyanate groups" or "cyanate groups") directly bonded to an aromatic ring in one molecule. The cyanate compound may be used alone or in combination of two or more.

[0161] Examples of such cyanate compounds include phenol novolac cyanate compounds, cresol novolac cyanate compounds, naphthalene ring-containing novolac cyanate compounds, allyl group-containing novolac cyanate compounds, naphthol aralkyl cyanate compounds, naphthol ether cyanate compounds, xylene resin cyanate compounds, bisphenol M cyanate compounds, bisphenol A cyanate compounds, diallyl bisphenol A cyanate compounds, bisphenol E cyanate compounds, bisphenol F cyanate compounds, and biphenyl aralkyl cyanate compounds. The cyanate ester compounds include bis(3,3-dimethyl-4-cyanophenyl)methane, 1,3-dicyanobenzene, 1,4-dicyanobenzene, 1,3,5-tricyanobenzene, 1,3-dicyanonaphthalene, 1,4-dicyanonaphthalene, 1,6-dicyanonaphthalene, 1,8-dicyanonaphthalene, 2,6-dicyanonaphthalene, 2,7-dicyanonaphthalene, 1,3,6-tricyanonaphthalene, 4,4'-dicyanobiphenyl, bis(4-cyanophenyl)ether, bis(4-cyanophenyl)sulfide and bis(4-cyanophenyl)sulfone. In addition, these cyanate ester compounds may be prepolymers or polymers of cyanate ester compounds.

[0162] Among them, the cyanate compound preferably contains one or more selected from the group consisting of phenol novolac type cyanate compounds, naphthol aralkyl type cyanate compounds, naphthol ether type cyanate compounds, xylene resin type cyanate compounds, bisphenol M type cyanate compounds, bisphenol A type cyanate compounds, diallyl bisphenol A type cyanate compounds, bisphenol E type cyanate compounds, bisphenol F type cyanate compounds, and biphenyl aralkyl type cyanate compounds, and prepolymers or polymers of these cyanate compounds, and more preferably naphthol aralkyl type cyanate compounds, from the viewpoint that the surface-coated titanium oxide (A) is more well dispersed, a resin composition having more excellent heat resistance and moisture absorption heat resistance and more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when cured, and an insulating layer having further suitable surface hardness can be obtained. Furthermore, when the resin composition contains these cyanate compounds, the adhesion with the surface-coating titanium oxide (A) is further improved, the aggregation of the surface-coating titanium oxide (A) in the resin composition can be further alleviated, the dispersibility is further improved, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance tend to be obtained.

[0163] As such a naphthol aralkyl type cyanate ester compound, a compound represented by formula (13) is more preferable.

[0164]

[0165] In formula (13), R 3 Each independently represents a hydrogen atom or a methyl group, and a hydrogen atom is preferred. In formula (13), n3 is an integer greater than or equal to 1, preferably an integer of 1 to 20, and more preferably an integer of 1 to 10.

[0166] As the bisphenol A type cyanate ester compound, one or more selected from the group consisting of 2,2-bis(4-cyanophenyl)propane and a prepolymer of 2,2-bis(4-cyanophenyl)propane may be used.

[0167] As such bisphenol A type cyanate compounds, commercially available products can be used, for example, Primaset (registered trademark) BADCy (trade name, Lonza KK, 2,2-bis(4-cyanophenyl)propane, cyanate group equivalent: 139 g / eq.) and CA210 (trade name, Mitsubishi Gas Chemical Co., Ltd., a prepolymer of 2,2-bis(4-cyanophenyl)propane, cyanate group equivalent: 139 g / eq.).

[0168] These cyanate compounds can also be produced according to known methods. As a specific production method, for example, the method described in Japanese Patent Application Laid-Open No. 2017-195334 (particularly paragraphs 0052 to 0057) can be cited.

[0169] Relative to a total of 100 parts by mass of the resin solid content in the resin composition, the content of the cyanate compound is preferably 1 to 65 parts by mass, more preferably 2 to 60 parts by mass, further preferably 3 to 55 parts by mass, further preferably 4 to 50 parts by mass, further preferably 5 to 45 parts by mass, further preferably, and particularly preferably 6 to 40 parts by mass. By making the content of the cyanate compound within the above range, the surface-coated titanium oxide (A) is further well dispersed, and a resin composition having further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained during curing, and further a tendency of an insulating layer having further suitable surface hardness can be obtained. By making the content of the cyanate compound within the above range, the surface-coated titanium oxide (A) is further well dispersed, and a resin composition having further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained during curing, and further a tendency of an insulating layer having further suitable surface hardness can be obtained. In addition, the adhesion with the surface-covering titanium oxide (A) is further improved, the aggregation of the surface-covering titanium oxide (A) in the resin composition can be further alleviated, the dispersibility is further improved, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and heat resistance tend to be obtained.

[0170] (Phenol compounds)

[0171] The resin composition of the present embodiment may include a phenol compound. If the phenol compound is a compound having two or more phenolic hydroxyl groups in one molecule, a known one may be used appropriately, and the type thereof is not particularly limited. One phenol compound may be used alone, or two or more phenol compounds may be used in combination.

[0172] As phenolic compounds, for example, cresol novolac type phenolic resin, biphenyl aralkyl type phenolic resin represented by formula (14), naphthol aralkyl type phenolic resin represented by formula (15), aminotriazine novolac type phenolic resin, naphthalene type phenolic resin, phenol novolac resin, alkylphenol novolac resin, bisphenol A type novolac resin, dicyclopentadiene type phenolic resin, xylok type phenolic resin, terpene modified phenolic resin and polyvinylphenol, etc. can be listed.

[0173] Among them, from the viewpoint of obtaining excellent moldability and surface hardness, the phenol compound preferably contains one or more selected from the group consisting of cresol novolac type phenolic resin, biphenyl aralkyl type phenolic resin represented by formula (14), naphthol aralkyl type phenolic resin represented by formula (15), aminotriazine novolac type phenolic resin and naphthalene type phenolic resin, and more preferably contains one or more selected from the group consisting of biphenyl aralkyl type phenolic resin represented by formula (14) and naphthol aralkyl type phenolic resin represented by formula (15).

[0174]

[0175] In formula (14), R 4 Each independently represents a hydrogen atom or a methyl group, and n4 is an integer of 1-10.

[0176]

[0177] In formula (15), R 5 Each independently represents a hydrogen atom or a methyl group, and n5 is an integer of 1-10.

[0178] The content of the phenol compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and still more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the phenol compound is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.

[0179] (Alkenyl-substituted nadic imide compound)

[0180] The resin composition of the present embodiment may include an alkenyl-substituted nadic imide compound. The alkenyl-substituted nadic imide compound is not particularly limited as long as it is a compound having one or more alkenyl-substituted nadic imide groups in one molecule. The alkenyl-substituted nadic imide compound may be used alone or in combination of two or more.

[0181] Examples of the alkenyl-substituted nadic acid imide compound include compounds represented by the following formula (2d).

[0182]

[0183] In formula (2d), R1 independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms (e.g., methyl or ethyl), and R2 represents an alkylene group having 1 to 6 carbon atoms, a phenylene group, a biphenylene group, a naphthylene group, or a group represented by formula (16) or formula (17).

[0184]

[0185] In formula (16), R3 represents methylene, isopropylidene, CO, O, S or SO2.

[0186]

[0187] In formula (17), R4 each independently represents an alkylene group having 1 to 4 carbon atoms or a cycloalkylene group having 5 to 8 carbon atoms.

[0188] The alkenyl-substituted nadic acid imide compound represented by formula (2d) may be a commercially available product or a product produced by a known method. Examples of commercially available products include BANI-M and BANI-X (these are trade names, Maruzen Petrochemical Co., Ltd.).

[0189] The content of the alkenyl-substituted nadic acid imide compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and even more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the alkenyl-substituted nadic acid imide compound is within the above range, there is a tendency for the adhesiveness, heat resistance, etc. to be more excellent.

[0190] (Oxetane resin)

[0191] The resin composition of the present embodiment may contain an oxetane resin. The oxetane resin is not particularly limited, and a generally known one may be used. The oxetane resin may be used alone or in combination of two or more.

[0192] Examples of the oxetane resin include oxetane, 2-methyloxetane, 2,2-dimethyloxetane, 3-methyloxetane, 3,3-dimethyloxetane and other alkyloxetanes; 3-methyl-3-methoxymethyloxetane, 3,3-bis(trifluoromethyl)perfluorooxetane, 2-chloromethyloxetane, 3,3-bis(chloromethyl)oxetane, biphenyl-type oxetane, OXT-101 (trade name, TOAGOSEI CO., LTD.) and OXT-121 (trade name, TOAGOSEI CO., LTD.) and the like.

[0193] The content of the oxetane resin is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and still more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the oxetane resin is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.

[0194] (Benzoxazine compounds)

[0195] The resin composition of the present embodiment may include a benzoxazine compound. As the benzoxazine compound, there is no particular limitation if it is a compound having two or more dihydrobenzoxazine rings in one molecule, and generally known compounds can be used. The benzoxazine compound can be used alone or in combination of two or more.

[0196] Examples of the benzoxazine compound include bisphenol A-type benzoxazine BA-BXZ, bisphenol F-type benzoxazine BF-BXZ, and bisphenol S-type benzoxazine BS-BXZ (these are trade names, KONISHI CHEMICAL IND CO., LTD.).

[0197] The content of the benzoxazine compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and even more preferably 10 to 30 parts by mass relative to 100 parts by mass of the total resin solid content in the resin composition. When the content of the benzoxazine compound is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.

[0198] (Compound having a polymerizable unsaturated group)

[0199] The resin composition of the present embodiment may include a compound having a polymerizable unsaturated group. As the compound having a polymerizable unsaturated group, there is no particular limitation, and generally known ones can be used. The compound having a polymerizable unsaturated group can be used alone or in combination of two or more.

[0200] Examples of the compound having a polymerizable unsaturated group include vinyl compounds such as ethylene, propylene, styrene, divinylbenzene and divinylbiphenyl; (meth)acrylates of monohydric or polyhydric alcohols such as methyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate and dipentaerythritol hexa(meth)acrylate; epoxy (meth)acrylates such as bisphenol A epoxy (meth)acrylate and bisphenol F epoxy (meth)acrylate; and benzocyclobutene resins.

[0201] The content of the compound having a polymerizable unsaturated group is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and further preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. By making the content of the compound having a polymerizable unsaturated group within the above range, there is a tendency for better adhesion, flexibility, etc.

[0202] <Filling material (C)>

[0203] For the resin composition containing surface-covered titanium oxide (A) and thermosetting compound (B), there is a further good dispersibility with surface-covered titanium oxide (A), and it is possible to obtain a resin composition having further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when solidified, the resin composition of the present embodiment preferably further includes a filler (C) different from the surface-covered titanium oxide (A). If the filler (C) is different from the surface-covered titanium oxide (A), there is no particular restriction. One filler (C) can be used alone, or two or more can be used in combination.

[0204] The average particle size (D50) of the filler (C) is preferably 0.10 to 10.0 μm, more preferably 0.30 to 5.0 μm. If the average particle size (D50) is within the above range, there is a tendency to obtain a resin composition having a further good dispersibility with the surface-covered titanium oxide (A) in a resin composition containing the surface-covered titanium oxide (A) and the thermosetting compound (B), and having a further excellent heat resistance and hygroscopic heat resistance during curing and a further excellent dielectric property (high dielectric constant and low dielectric loss tangent). The average particle size (D50) of the filler (C) can be calculated in the same manner as the average particle size (D50) of the surface-covered titanium oxide (A).

[0205] Examples of the filler (C) include silicon dioxide, silicon compounds (e.g., white carbon), metal oxides (e.g., aluminum oxide, titanium dioxide, strontium titanate (SrTiO3), calcium titanate (CaTiO3), titanium oxide (TiO2) different from the surface-coated titanium oxide (A), MgSiO4, MgTiO3, ZnTiO3, ZnTiO4, CaTiO3, SrTiO3, SrZrO3, BaTi2O5, BaTi4O9, Ba2Ti9O 20 、Ba(Ti,Sn)9O 20 , ZrTiO4, (Zr,Sn)TiO4, BaNd2Ti5O 14 、BaSmTiO 14, Bi2O3-BaO-Nd2O3-TiO2, La2Ti2O7, barium titanate (BaTiO3), Ba(Ti,Zr)O3, (Ba,Sr)TiO3, molybdenum compounds (such as molybdic acid, zinc molybdates such as ZnMoO4 and Zn3Mo2O9, ammonium molybdate, sodium molybdate, potassium molybdate, calcium molybdate, molybdenum disulfide, molybdenum trioxide, molybdic acid hydrate, zinc ammonium molybdate hydrates such as (NH4)Zn2Mo2O9·(H3O)), zinc oxide, magnesium oxide and zirconium oxide, etc.), metal nitrides (such as boron nitride, silicon nitride and aluminum nitride, etc.), metal sulfur oxides (such as barium sulfate, etc.), metal hydroxides (such as aluminum hydroxide, aluminum hydroxide heat-treated products (such as aluminum hydroxide is heated to remove part of the crystal water), boehmite and magnesium hydroxide, etc.), zinc compounds (such as boric acid The invention also includes inorganic fillers such as zinc, zinc stannate, etc.), clay, kaolin, talc, calcined clay, calcined kaolin, mica, E-glass, A-glass, NE-glass, C-glass, L-glass, D-glass, S-glass, M-glass G20, glass short fibers (including glass powders of E-glass, T-glass, D-glass, S-glass and Q-glass), hollow glass, spherical glass, and metal particles with insulation treatment for metals such as gold, silver, palladium, copper, nickel, iron, cobalt, zinc, Mn-Mg-Zn series, Ni-Zn series, Mn-Zn series, carbonyl iron, Fe-Si series, Fe-Al-Si series, and Fe-Ni series; rubber powders of styrene type, butadiene type and acrylic type; core-shell type rubber powder; silicone resin powder; silicone rubber powder; silicone composite powder and other organic fillers.

[0206] Among them, the filler (C) preferably contains one or more selected from the group consisting of silica, alumina, barium titanate, strontium titanate, calcium titanate, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and silicone composite powder, more preferably one or more selected from the group consisting of silica, talc, and zinc molybdate, and further preferably contains silica, from the viewpoint of having further good dispersibility with the surface-covered titanium oxide (A) in the resin composition containing the surface-covered titanium oxide (A) and the thermosetting compound (B), and having further excellent heat resistance and moisture absorption heat resistance when cured, and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent).

[0207] As silicon dioxide, for example, natural silicon dioxide, fused silica, synthetic silica, fumed silica and hollow silica etc. can be listed. If the resin composition includes silicon dioxide, there is a tendency that processability is more excellent. These silicon dioxides can be used alone or in combination of two or more. Among them, for the viewpoint of having low thermal expansion coefficient and excellent dispersibility in the resin composition, it is preferably selected from more than one of the group consisting of fused silica and hollow silica.

[0208] As the silica, commercially available products may be used, and examples thereof include SC2050-MB, SC5050-MOB, SC2500-SQ, SC4500-SQ, SC4053-SQ, and SC5050-MOB (these, trade names, ADMATECHS COMPANY LIMITED); and SFP-130MC (trade name, DENKA CORPORATION).

[0209] The filler (C) may also be a surface-treated filler having an inorganic oxide formed on at least a portion of the surface of the filler core particle. Such a filler may include, for example, surface-treated molybdenum compound particles (supported type) having an inorganic oxide formed on at least a portion of the surface of the core particle composed of a molybdenum compound.

[0210] For inorganic oxide, at least a portion of the surface of the filler core particles is imparted. Inorganic oxide can be partially imparted on the surface of the filler core particles, or it can be imparted in a manner that coats the entire surface of the filler core particles. From the viewpoint of obtaining a printed circuit board with better heat resistance and hygroscopic heat resistance and better dielectric properties (high dielectric constant and low dielectric loss tangent), inorganic oxide is preferably uniformly imparted in a manner that coats the entire surface of the filler core particles, i.e., preferably uniformly forming a film of inorganic oxide on the surface of the filler core particles.

[0211] Inorganic oxide is preferably excellent in heat resistance, and its type is not particularly limited, and is more preferably metal oxide. As metal oxide, for example, SiO2, Al2O3, TiO2, ZnO, In2O3, SnO2, NiO, CoO, V2O5, CuO, MgO, and ZrO2 can be listed. They can be used alone or in combination of two or more. Among them, from the viewpoint of heat resistance, insulating properties and cost, it is preferably selected from more than one of the group consisting of silicon dioxide (SiO2), titanium dioxide (TiO2), aluminum oxide (Al2O3) and zirconium oxide (ZrO2), more preferably silicon dioxide.

[0212] The thickness of the inorganic oxide on the surface can be appropriately set according to the desired performance, without particular limitation. From the viewpoints of being able to form a uniform inorganic oxide coating, being more excellent in adhesion to the filler core particles, being able to obtain a printed circuit board with better heat resistance and hygroscopic heat resistance and better dielectric properties (high dielectric constant and low dielectric loss tangent), etc., its thickness is preferably 3 to 500 nm, more preferably 5 to 200 nm, and further preferably 10 to 100 nm.

[0213] Examples of the surface-treated molybdenum particles (supported type) include particles of a molybdenum compound surface-treated with a silane coupling agent, or particles surface-treated with an inorganic oxide by a sol-gel method or a liquid phase precipitation method.

[0214] As the surface-treated molybdenum compound particles, it is preferred that an inorganic oxide is imparted to at least a portion of the surface of the core particle composed of the molybdenum compound or the entire surface, that is, to at least a portion of the periphery of the core particle or the entire periphery. In such surface-treated molybdenum compound particles, it is more preferred that silicon dioxide is imparted as an inorganic oxide to at least a portion of the surface of the core particle composed of the molybdenum compound or the entire surface, that is, to at least a portion of the periphery of the core particle or the entire periphery. The core particle composed of the molybdenum compound is more preferably at least one selected from the group consisting of molybdic acid, zinc molybdate, and zinc ammonium molybdate hydrate, and is further preferably zinc molybdate.

[0215] From the viewpoint of dispersibility in the resin composition, the average particle size (D50) of the surface-treated molybdenum compound particles is preferably 0.1 to 10 μm, more preferably 0.5 to 8 μm, further preferably 1 to 4 μm, and further preferably 1 to 3 μm. The average particle size (D50) of the surface-treated molybdenum compound particles can be calculated in the same manner as the average particle size (D50) of the surface-coated titanium oxide (A).

[0216] The core particles composed of the molybdenum compound can be produced by various known methods such as a pulverization method and a granulation method, and the production method is not particularly limited. In addition, commercially available products can also be used.

[0217] The method for producing the surface-treated molybdenum compound particles is not particularly limited, and the surface-treated molybdenum compound particles can be obtained by appropriately using various known methods such as sol-gel method, liquid phase precipitation method, dip coating method, spray coating method, printing method, chemical plating method, sputtering method, evaporation method, ion plating method and CVD method, and imparting an inorganic oxide or its precursor to the surface of the core particle composed of the molybdenum compound. The method for imparting an inorganic oxide or its precursor to the surface of the core particle composed of the molybdenum compound can be any of a wet method and a dry method.

[0218] As a suitable method for manufacturing surface-treated molybdenum compound particles, for example, a molybdenum compound (core particle) is dispersed in an alcohol solution in which metal alkoxides such as silicon alkoxides (alkoxysilanes) and aluminum alkoxides are dissolved, and a mixed solution of water, alcohol and a catalyst is added dropwise while stirring to hydrolyze the alkoxide, thereby forming a film of silicon oxide or aluminum oxide on the surface of the compound in the form of a low-refractive index film, and then the obtained powder is subjected to solid-liquid separation, and a heat treatment is performed after vacuum drying. As other suitable manufacturing methods, for example, a molybdenum compound (core particle) is dispersed in an alcohol solution in which metal alkoxides such as silicon alkoxides and aluminum alkoxides are dissolved, mixed at high temperature and low pressure, a film of silicon oxide or aluminum oxide is formed on the surface of the compound, and then the obtained powder is subjected to vacuum drying and pulverization. By these methods, surface-treated molybdenum compound particles having a film of metal oxides such as silicon dioxide and aluminum oxide on the surface of the molybdenum compound can be obtained.

[0219] From the viewpoint of having a further good dispersibility with the surface-covered titanium oxide (A) in the resin composition containing the surface-covered titanium oxide (A) and the thermosetting compound (B), and obtaining a resin composition having further excellent heat resistance and hygroscopic heat resistance and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when cured, the content of the filler (C) is preferably 50 to 300 parts by mass, more preferably 70 to 200 parts by mass, and further preferably 100 to 150 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When two or more fillers (C) are contained, the total amount may be within the above range.

[0220] In terms of volume ratio (surface-coated titanium oxide (A): filler (C)), it is preferred that the surface-coated titanium oxide (A) and filler (C) are included in the range of 15:85 to 85:15, more preferably in the range of 20:80 to 80:20, and further preferably in the range of 25:75 to 75:25. If the volume ratio is in the above range, there is a tendency for the surface-coated titanium oxide (A) and filler (C) to be better dispersed in the thermosetting compound (B). Therefore, in a resin composition such as a resin varnish, the surface-coated titanium oxide (A) and filler (C) are not unevenly distributed, so that the water absorption based on titanium oxide is further suppressed, and a printed circuit board having better heat resistance and hygroscopic heat resistance and better dielectric properties (high dielectric constant and low dielectric loss tangent) during curing can be obtained, and an insulating layer having further excellent hygroscopic heat resistance can be obtained. In addition, a molded product having excellent coating properties and good appearance can also be obtained. In addition, in the resin composition, since the surface-coated titanium oxide (A) and the filler (C) are well dispersed, the thermal expansion coefficient of the insulating layer can be appropriately controlled, and a dielectric path can be efficiently formed. Therefore, there is a tendency to appropriately obtain an insulating layer having excellent moisture absorption heat resistance and low thermal expansion coefficient, and having a high dielectric constant and a low dielectric loss tangent.

[0221] In addition, in the resin composition of the present embodiment, from the viewpoint of miniaturization of the circuit and high capacitance of the capacitor, which contributes to miniaturization of high-frequency electronic components, the filler (C) can use a filler having a high dielectric constant. Examples of such fillers include titanium oxide (TiO2) different from the surface-coated titanium oxide (A), MgSiO4, MgTiO3, ZnTiO3, ZnTiO4, CaTiO3, SrTiO3, SrZrO3, BaTi2O5, Ba2Ti9O 20 、Ba(Ti,Sn)9O 20 , ZrTiO4, (Zr,Sn)TiO4, BaNd2Ti5O 14 、BaSmTiO 14 , Bi2O3-BaO-Nd2O3-TiO2, La2Ti2O7, BaTiO3, Ba(Ti,Zr)O3 and (Ba,Sr)TiO3, and metal particles obtained by insulating gold, silver, palladium, copper, nickel, iron, cobalt, zinc, Mn-Mg-Zn series, Ni-Zn series, Mn-Zn series, carbonyl iron, Fe-Si series, Fe-Al-Si series and Fe-Ni series. These fillers can be used alone or in combination of two or more.

[0222] <Silane coupling agent>

[0223] The resin composition of the present embodiment may further include a silane coupling agent. The resin composition contains a silane coupling agent, which has a tendency to further improve the dispersibility of the surface-covered titanium oxide (A) and the filler (C) compounded as needed in the resin composition, and further improve the bonding strength between the components contained in the resin composition and the substrate described later. The silane coupling agent can be used alone or in combination of two or more.

[0224] As a silane coupling agent, there is no particular limitation, and a silane coupling agent commonly used for surface treatment of inorganic substances can be used. For example, aminosilane compounds (such as 3-aminopropyl triethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, etc.), epoxy silane compounds (such as 3-glycidoxypropyl trimethoxysilane, etc.), acrylic silane compounds (such as γ-acryloxypropyl trimethoxysilane, etc.), cationic silane compounds (such as N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyl trimethoxysilane hydrochloride, etc.), styryl silane compounds, phenyl silane compounds, etc. can be listed. Silane coupling agent can be used alone or in combination of two or more. Among them, the silane coupling agent is preferably selected from one or more of the group consisting of epoxy silane compounds and styryl silane compounds. Examples of epoxy silane compounds include KBM-403, KBM-303, KBM-402, and KBE-403 (trade names, Shin-Etsu Chemical Co., Ltd.) Examples of styrene silane compounds include KBM-1403 (trade name, Shin-Etsu Chemical Co., Ltd.) and the like.

[0225] The content of the silane coupling agent is not particularly limited, and may be 0.1 to 5.0 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.

[0226] <Wetting and dispersing agent>

[0227] The resin composition of the present embodiment may further contain a wetting dispersant. The resin composition containing a wetting dispersant tends to further improve the dispersibility of the filler (C). The wetting dispersant may be used alone or in combination of two or more.

[0228] The wetting dispersant may be a known dispersant (dispersion stabilizer) for dispersing the filler (C), and examples thereof include DISPER BYK (registered trademark)-110, 111, 118, 180, 161, 2009, 2152, 2155, W996, W9010, and W903 (these are trade names, BYK Japan KK).

[0229] The content of the wetting and dispersing agent is not particularly limited, but is preferably 0.5 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the total resin solid content in the resin composition.

[0230] <Curing Accelerator>

[0231] The resin composition of the present embodiment may further contain a curing accelerator. The curing accelerator may be used alone or in combination of two or more.

[0232] Examples of the curing accelerator include imidazoles such as triphenylimidazole (e.g., 2,4,5-triphenylimidazole); organic peroxides such as benzoyl peroxide, lauroyl peroxide, acetyl peroxide, p-chlorobenzoyl peroxide, and di-tert-butyl diperphthalate; azo compounds such as azobisnitrile; N,N-dimethylbenzylamine, N,N-dimethylaniline, N,N-dimethyltoluidine, 2-N-ethylphenylaminoethanol, tri-n-butylamine, pyridine, quinoline, N-methylmorpholine, triethanolamine, triethylenediamine, tetramethylbutylenediamine, N-methyl Tertiary amines such as tertiary amines such as methylpiperidine; phenols such as phenol, xylenol, cresol, resorcinol, and catechol; organic metal salts such as lead naphthenate, lead stearate, zinc naphthenate, zinc octoate, manganese octoate, tin oleate, dibutyltin maleate, manganese naphthenate, cobalt naphthenate, and ferric acetylacetonate; those obtained by dissolving these organic metal salts in hydroxyl-containing compounds such as phenol and bisphenol; inorganic metal salts such as tin chloride, zinc chloride, and aluminum chloride; organic tin compounds such as dioctyltin oxide, other alkyl tins, and alkyl tin oxides; phosphorus compounds such as triphenylphosphine and phosphonium borate compounds, etc. Among them, triphenylimidazoles such as 2,4,5-triphenylimidazole and manganese octoate are preferred because they tend to promote the curing reaction and further improve the glass transition temperature.

[0233] The content of the curing accelerator is not particularly limited, but may be 0.001 parts by mass or more and 1.0 parts by mass or less relative to 100 parts by mass of the total resin solid content in the resin composition.

[0234] <Solvent>

[0235] The resin composition of the present embodiment may further include a solvent. The resin composition contains a solvent, which has a tendency to reduce the viscosity during the preparation of the resin composition, further improve the operability (handling property), and further improve the impregnation property of the substrate. One solvent may be used alone, or two or more solvents may be used in combination.

[0236] The solvent is not particularly limited as long as it can dissolve part or all of the components in the resin composition, and examples thereof include ketones (acetone, methyl ethyl ketone, etc.), aromatic hydrocarbons (such as toluene, xylene, etc.), amides (such as dimethyl formaldehyde, etc.), propylene glycol monomethyl ether and its acetate, etc.

[0237] <Other ingredients>

[0238] The resin composition of the present embodiment may contain ingredients other than the above within the range that does not impair the desired properties. For example, as flame retardant compounds, bromine compounds such as 4,4'-dibromobiphenyl, phosphoric acid esters, melamine phosphate, melamine, nitrogen-containing compounds such as benzoguanamine, and silicon compounds, etc. can be cited. In addition, as various additives, there can be cited: ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, lubricants, defoamers, dispersants, leveling agents (surface conditioners), brighteners, inhibitors, etc.

[0239] The content of other components is not particularly limited, but is usually 0.01 parts by mass or more and 10 parts by mass or less, respectively, relative to 100 parts by mass of the total resin solid content in the resin composition.

[0240] [Method for producing resin composition]

[0241] The manufacture method of the resin composition of the present embodiment is not particularly limited, and for example, a method in which the surface-covered titanium oxide (A), a thermosetting compound (B) and the above-mentioned components that can be arbitrarily included as needed are mixed and fully stirred can be cited. At this time, in order to make each component dissolve or disperse uniformly, known treatments such as stirring, mixing, and kneading treatment can be implemented. Specifically, stirring and dispersing treatment is implemented by using a stirring tank equipped with a stirrer with appropriate stirring ability, which can improve the dispersibility of the surface-covered titanium oxide (A) and the filler (C) compounded as needed in the resin composition. The above-mentioned stirring, mixing, and kneading treatment can be appropriately implemented using known devices such as ball mills, bead mills, etc. for the purpose of mixing, or mixing devices of revolution or autogenous type.

[0242] In addition, when preparing the resin composition, a solvent can be used as needed to prepare a resin varnish. The type of solvent is not particularly limited as long as it can dissolve the resin in the resin composition. Specific examples are as described above. The resin varnish can usually be obtained by adding 10 to 900 parts by mass of a solvent to 100 parts by mass of the components other than the solvent in the resin composition and performing the aforementioned known treatments (stirring, mixing and kneading treatments, etc.). The type of solvent is not particularly limited as long as it can dissolve the resin in the resin composition. Specific examples are as described above.

[0243] 〔use〕

[0244] The resin composition of the present embodiment can be suitably used as a raw material for a cured product, a prepreg, a film-like underfill material, a resin sheet, a laminate, a build-up material, a non-conductive film, a metal foil-clad laminate, a printed circuit board, and a fiber-reinforced composite material, or can be suitably used in the manufacture of a semiconductor device. These are described below.

[0245] 〔Cured product〕

[0246] The cured product is obtained by curing the resin composition of the present embodiment. As a method for manufacturing a cured product, for example, the resin composition of the present embodiment can be melted or dissolved in a solvent (solvent), poured into a mold, and cured under normal conditions using heat, light, etc. to obtain it. During thermal curing, the curing temperature is preferably within the range of 120 to 300° C. from the viewpoint that curing is carried out efficiently and deterioration of the obtained cured product is prevented.

[0247] 〔Prepreg〕

[0248] The prepreg of the present embodiment contains a substrate, and a resin composition of the present embodiment impregnated or coated on the substrate. The prepreg of the present embodiment can be obtained, for example, by semi-curing (B-stage) the resin composition of the present embodiment (e.g., uncured state (A stage)) after being impregnated or coated on the substrate, and then drying at 120 to 220 ° C for about 2 to 15 minutes. At this time, the amount of adhesion of the resin composition (also including the cured product of the resin composition) to the substrate, that is, the amount of the resin composition (including the surface-covered titanium oxide (A) and the filler (C) compounded as needed) relative to the total amount of the semi-cured prepreg is preferably in the range of 20 to 99% by mass. It should be noted that the semi-cured state (B stage) refers to the state that the components contained in the resin composition have not yet actively started to react (cured), but the resin composition is in a dry state, that is, the state in which the solvent is volatilized to the extent of no adhesion by heating, and also includes the state in which the solvent is only volatilized without heating or curing. In the present embodiment, the minimum melt viscosity of the semi-cured state (B stage) is usually less than 20,000 Pa·s. The lower limit of the minimum melt viscosity is, for example, above 10 Pa·s. It should be noted that, in the present embodiment, the minimum melt viscosity is measured using the following method. That is, using 1 g of resin powder collected from the resin composition as a sample, the minimum melt viscosity is measured using a rheometer (ARES-G2 (trade name), TA Instruments). Here, a disposable plate with a plate diameter of 25 mm is used to measure the minimum melt viscosity of the resin powder in a range of above 40°C and below 180°C, at a heating rate of 2°C / min, a frequency of 10.0 rad / sec, and a strain of 0.1%.

[0249] As a substrate, if it is a substrate used for various printed circuit board materials, there is no particular restriction. As the material of the substrate, for example, glass fiber (such as E-glass, D-glass, L-glass, S-glass, T-glass, Q-glass, UN-glass and NE-glass, etc.), inorganic fibers other than glass fiber (such as quartz, etc.), organic fibers (such as polyimide, polyamide, polyester, liquid crystal polyester and polytetrafluoroethylene, etc.) can be cited. As the form of the substrate, there is no particular restriction, and it can be cited: woven fabric, non-woven fabric, roving, chopped strand mat and surface processing mat, etc. These substrates can be used alone or in combination with more than two kinds. Among these substrates, from the viewpoint of dimensional stability, it is preferably a woven fabric that has been subjected to super fiber opening treatment and hole filling treatment, and from the viewpoint of hygroscopic heat resistance, it is preferably a glass fabric that has been subjected to surface treatment using silane coupling agents, etc., such as epoxy silane treatment and amino silane treatment. From the viewpoint of having excellent dielectric properties, it is preferably glass fibers such as E-glass, L-glass, NE-glass and Q-glass.

[0250] 〔Resin sheet〕

[0251] The resin sheet of the present embodiment includes the resin composition of the present embodiment. The resin sheet can also be made into a resin sheet provided with a support body including a support body and a layer formed by the resin composition of the present embodiment disposed on the surface of the support body. The resin sheet can be used as a laminated film or a dry film solder resist. As a method for manufacturing the resin sheet, there is no particular limitation, for example, the following method can be cited: a solution obtained by dissolving the resin composition of the present embodiment in a solvent is applied (coated) to a support body and dried to obtain a resin sheet.

[0252] Examples of the support include polyethylene film, polypropylene film, polycarbonate film, polyethylene terephthalate film, ethylene tetrafluoroethylene copolymer film, release film obtained by coating a release agent on the surface of these films, organic film substrates such as polyimide film, conductor foils such as copper foil and aluminum foil, glass plates, SUS plates, FRP and the like, without particular limitation.

[0253] The coating method (coating method) can be, for example, a method in which a solution obtained by dissolving the resin composition of the present embodiment in a solvent is applied to a support by a rod coater, a die coater, a scraper, a Baker applicator, etc. In addition, a single-layer sheet (resin sheet) can be prepared by peeling off or etching the support from a resin sheet provided with a support on which a support and a resin composition are stacked after drying. It should be noted that a single-layer sheet (resin sheet) can be obtained by supplying a solution obtained by dissolving the resin composition of the present embodiment in a solvent to a mold having a sheet-shaped mold groove, drying, etc. to form a sheet, without using a support.

[0254] It should be noted that in the preparation of the single-layer sheet or the resin sheet with a support according to the present embodiment, there is no particular restriction on the drying conditions when removing the solvent. From the viewpoint of easily removing the solvent from the resin composition and inhibiting the progress of curing during drying, it is preferably dried at a temperature of 20 to 200°C for 1 to 90 minutes. In addition, in the single-layer sheet or the resin sheet with a support, the resin composition can be used in an uncured state where only the solvent is dried, or it can be used in a semi-cured (B-stage) state as needed. In addition, the thickness of the resin layer of the single-layer sheet or the resin sheet with a support related to the present embodiment can be adjusted by the concentration of the solution of the resin composition of the present embodiment and the coating thickness, and there is no particular restriction. From the viewpoint of easily removing the solvent during drying, it is preferably 0.1 to 500 μm.

[0255] 〔Laminated board〕

[0256] The laminate of the present embodiment includes one or more of the group consisting of the prepreg and resin sheet of the present embodiment. For prepreg and resin sheet, when more than two kinds are stacked, the resin composition used by each prepreg and resin sheet can be the same or different. In addition, when using both prepreg and resin sheet, the resin composition used in them can be the same or different. In the laminate of the present embodiment, one or more of the group consisting of prepreg and resin sheet can be semi-cured state (B stage), or can be fully cured state (C stage).

[0257] [Metal foil-clad laminate]

[0258] The metal foil-clad laminated plate of the present embodiment includes the laminated plate of the present embodiment and a metal foil disposed on one surface or both surfaces of the laminated plate.

[0259] The metal foil-clad laminate may include at least one prepreg according to the present embodiment and a metal foil laminated on one or both surfaces of the prepreg.

[0260] Furthermore, the metal foil-clad laminate may include at least one resin sheet of the present embodiment and a metal foil laminated on one or both surfaces of the resin sheet.

[0261] In the metal foil clad laminate of the present embodiment, the resin compositions used in the prepregs and the resin sheets may be the same or different, and when both the prepregs and the resin sheets are used, the resin compositions used in them may be the same or different. In the metal foil clad laminate of the present embodiment, one or more selected from the group consisting of the prepregs and the resin sheets may be in a semi-cured state or in a fully cured state.

[0262] In the metal foil clad laminate of the present embodiment, the metal foil is laminated on one or more selected from the group consisting of the prepreg of the present embodiment and the resin sheet of the present embodiment, wherein the metal foil is preferably laminated in a manner that the metal foil contacts the surface of one or more selected from the group consisting of the prepreg of the present embodiment and the resin sheet of the present embodiment. "Laminated in a manner that the metal foil contacts the surface of one or more selected from the group consisting of the prepreg and the resin sheet" means that there is no layer such as an adhesive layer between the prepreg or the resin sheet and the metal foil, and the prepreg or the resin sheet is in direct contact with the metal foil. As a result, there is a tendency that the metal foil peel strength of the metal foil clad laminate becomes higher and the insulation reliability of the printed circuit board is improved.

[0263] The metal foil clad laminate of the present embodiment may have a prepreg and / or resin sheet of the present embodiment overlapped with more than one sheet, and a metal foil disposed on one or both sides of the prepreg and / or resin sheet. As a method for manufacturing the metal foil clad laminate of the present embodiment, for example, a method of overlapping more than one sheet of the prepreg and / or resin sheet of the present embodiment, disposing metal foil on one or both sides thereof and performing stacking molding can be cited. As a molding method, a method commonly used when molding laminates and multilayer boards for printed circuit boards can be cited. In more detail, a multistage press, a multistage vacuum press, a continuous molding machine, an autoclave molding machine, etc. can be cited, at a temperature of about 180 to 350°C, a heating time of about 100 to 300 minutes, and a surface pressure of 20 to 100 kgf / cm 2 A method of stacking molding from left to right and bottom to bottom.

[0264] In addition, a multilayer board can also be made by combining the prepreg and / or resin sheet of the present embodiment with a separately made inner layer circuit board and stacking molding. As a manufacturing method of a multilayer board, for example, a multilayer board can be made as follows: after arranging copper foil with a thickness of about 35 μm on both sides of the prepreg and / or resin sheet of the present embodiment with more than one overlap, and stacking and forming a copper foil-clad laminate by the above-mentioned molding method, an inner layer circuit is formed, and a blackening treatment is applied to the circuit to form an inner layer circuit board, and then, the inner layer circuit board and the prepreg and / or resin sheet of the present embodiment are alternately arranged piece by piece, and then copper foil is arranged in the outermost layer, and stacking molding is performed under the above-mentioned conditions, preferably under vacuum. The metal foil-clad laminate of the present embodiment can be suitably used as a printed circuit board.

[0265] (metal foil)

[0266] There are no particular restrictions on the metal foil, and examples thereof include gold foil, silver foil, copper foil, tin foil, nickel foil, and aluminum foil. Among them, copper foil is preferred. If the copper foil is used as a material for a common printed circuit board, there are no particular restrictions, and examples thereof include rolled copper foil and electrolytic copper foil. Among them, electrolytic copper foil is preferred from the perspective of copper foil peel strength and the formability of fine wiring. The thickness of the copper foil is not particularly limited, and may be about 1.5 to 70 μm.

[0267] 〔Printed circuit board〕

[0268] The printed circuit board of the present embodiment has an insulating layer and a conductor layer disposed on one or both sides of the insulating layer, and the insulating layer comprises a cured product of the resin composition of the present embodiment. The insulating layer preferably comprises at least one of a layer (a layer comprising a cured product) formed by the resin composition of the present embodiment and a layer (a layer comprising a cured product) formed by a prepreg. Such a printed circuit board can be manufactured by a common method, and its manufacturing method is not particularly limited, for example, the above-mentioned metal foil laminate can be used to manufacture. Below, an example of a method for manufacturing a printed circuit board is illustrated.

[0269] First, prepare the above-mentioned metal foil-clad laminate. Then, the surface of the metal foil-clad laminate is subjected to etching treatment to form the inner layer circuit and make the inner layer substrate. The inner layer circuit surface of the inner layer substrate is subjected to surface treatment for improving the bonding strength as needed, and then the required number of prepregs are overlapped on the inner layer circuit surface, and then the metal foil for the outer layer circuit is stacked on its outside, and heated and pressed and formed into one. In this way, a multilayer laminate having an insulating layer composed of a cured product of a substrate and the resin composition of the present embodiment is formed between the metal foil for the inner layer circuit and the outer layer circuit. Then, after the opening processing for through holes (through holes) and guide holes (via holes) is performed on the multilayer laminate, a plated metal film that makes the inner layer circuit and the metal foil for the outer layer circuit conductive is formed on the wall surface of the hole, and then the metal foil for the outer layer circuit is subjected to etching treatment to form the outer layer circuit, thereby manufacturing a printed circuit board.

[0270] The printed wiring board obtained in the above manufacturing example has the following structure: it has an insulating layer and a conductor layer formed on the surface of the insulating layer, and the insulating layer contains the cured product of the resin composition of this embodiment. That is, the prepreg of this embodiment (including the base material and the cured product of the resin composition of this embodiment impregnated or coated thereon) and the layer of the resin composition of the metal foil-clad laminate of this embodiment (the layer containing the cured product of the resin composition of this embodiment) are composed of the insulating layer containing the cured product of the resin composition of this embodiment.

[0271] 〔Semiconductor devices〕

[0272] The semiconductor device can be manufactured by mounting a semiconductor chip on a conductive position of the printed circuit board of this embodiment. Here, the conductive position refers to a position in a multilayer printed circuit board where an electrical signal is transmitted, and the position may be a surface or an embedded position. In addition, the semiconductor chip is not particularly limited as long as it is an electrical circuit component made of semiconductor.

[0273] There are no particular restrictions on the method of mounting semiconductor chips when manufacturing semiconductor devices as long as the semiconductor chips function effectively. Specifically, there are wire bonding mounting methods, flip chip mounting methods, mounting methods based on bumpless build-up layers (BBUL), mounting methods based on anisotropic conductive films (ACF), and mounting methods based on non-conductive films (NCF).

[0274] Example

[0275] Hereinafter, the present embodiment will be described in more detail using examples and comparative examples. The present embodiment is not limited in any way by the following examples.

[0276] [Method for measuring average particle size]

[0277] The average particle diameter (D50) of the surface-coating titanium oxide and the filler (fused spherical silica) was calculated by measuring the particle size distribution by a laser diffraction / scattering method using a laser diffraction / scattering particle size distribution measuring apparatus (Microtrac MT3300EXII (trade name), Microtrac BEL) under the following measurement conditions.

[0278] (Measurement conditions of laser diffraction / scattering particle size distribution measuring device)

[0279] (Surface covered with titanium oxide)

[0280] Solvent: methyl ethyl ketone, solvent refractive index: 1.33, particle refractive index: 2.72, transmittance: 85±5%.

[0281] (Filling material)

[0282] Solvent: methyl ethyl ketone, solvent refractive index: 1.33, particle refractive index: 1.45 (fused spherical silica), transmittance: 85±5%.

[0283] [Method for measuring weight loss rate of surface-covered titanium oxide]

[0284] The weight loss rate (%) of the surface-coated titanium oxide when heated from 30°C to 300°C at a heating rate of 10°C / min was measured by the following method. First, using a differential thermal thermogravimetric synchronous measuring device (TG-DSC, NEXTA STA200 (trade name), Hitachi High-Tech Science Corporation), each weighed surface-coated titanium oxide was placed in an aluminum pan, and the weight loss rate when heated from 30°C to 300°C at a heating rate of 10°C / min was measured. The results are shown in Table 1.

[0285] [Synthesis Example 1] Synthesis of naphthol aralkyl cyanate compound (SN495V-CN)

[0286] 300 g (1.28 mol in terms of OH group) of naphthol aralkyl phenol resin (SN495V (trade name), OH group (hydroxyl) equivalent: 236 g / eq., NIPPONSTEEL Chemical & Material Co., Ltd.) and 194.6 g (1.92 mol) of triethylamine (1.5 mol per 1 mol of hydroxyl group) were dissolved in 1800 g of dichloromethane to prepare solution 1. 125.9 g (2.05 mol) of cyanogen chloride (1.6 mol per 1 mol of hydroxyl group), 293.8 g of dichloromethane, 194.5 g (1.92 mol) of 36% hydrochloric acid (1.5 mol per 1 mol of hydroxyl group) and 1205.9 g of water were added to solution 1 over 30 minutes while stirring and maintaining the liquid temperature at -2 to -0.5°C. After the injection of solution 1 is completed, the mixture is stirred at the same temperature for 30 minutes, and then a solution (solution 2) in which 65 g (0.64 mol) of triethylamine (0.5 mol relative to 1 mol of hydroxyl group) is dissolved in 65 g of dichloromethane is injected over a period of 10 minutes. After the injection of solution 2 is completed, the reaction is terminated by stirring at the same temperature for 30 minutes. Then, the reaction solution is allowed to stand and the organic phase and the aqueous phase are separated, and the obtained organic phase is washed 5 times with 1300 g of water. The conductivity of the wastewater after the fifth washing is 5 μS / cm, confirming that the ionic compounds that can be removed by washing with water have been fully removed. The organic phase after washing is concentrated under reduced pressure, and finally concentrated to dryness at 90°C for 1 hour to obtain the target naphthol aralkyl type cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq., R in the above formula (13) 3 All of them are hydrogen atoms, and n3 is an integer of 1 to 10) (orange viscous material) 331 g. The infrared absorption spectrum of the obtained SN495V-CN shows 2250 cm -1 The absorption of the cyanate group is not shown, and the absorption of the hydroxyl group is not shown.

[0287] [Example 1]

[0288] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name, K.I. Chemical Industry Co., LTD.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name, Nippon Kayaku Co., Ltd.), 28 parts by mass of a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Corporation, a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, surface-covered titanium oxide (crystal structure: rutile type, titanium dioxide is surface-treated with silica, alumina and dimethyl silicone (total content of silica, alumina and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass, average particle size (D50): 0.21 μm, CR-63 (trade name), ISHIHARA SANGYO A resin varnish was obtained by mixing 80 parts by mass of molten spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, ADMATECHS COMPANY LIMITED), 120 parts by mass of silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK JAPAN KK), 2 parts by mass of wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK JAPAN KK), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0289] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg and pressed at a surface pressure of 30 kgf / cm 2 The laminate was then vacuum pressed at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.

[0290] [Example 2]

[0291] 8 parts by mass of the naphthol aralkyl type cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name, K.I.CHEMICAL INDUSTRY CO., LTD.), 28 parts by mass of a biphenyl aralkyl type maleimide compound (MIR-3000-70MT (trade name, Nippon Kayaku Co., Ltd.), 28 parts by mass of a naphthalene type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with alumina and organosilane (total content of alumina and organosilane: 2% by mass), titanium oxide content: 98% by mass, average particle size (D50): 0.40 μm, R-22L (trade name), SAKAI CHEMICAL INDUSTRY CO., LTD.), 80 parts by mass of molten spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, ADMATECHS COMPANY LIMITED), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK JAPAN KK), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK JAPAN KK), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0292] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg and pressed at a surface pressure of 30 kgf / cm 2 The laminate was then vacuum pressed at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.

[0293] [Example 3]

[0294] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name, K.I.CHEMICAL INDUSTRY CO., LTD.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name, Nippon Kayaku Co., Ltd.), 28 parts by mass of a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with alumina and silicone oil (total content of alumina and silicone oil: 2% by mass), titanium oxide content: 98% by mass, average particle size (D50): 0.20 μm, R-11P (trade name), SAKAI CHEMICAL INDUSTRY CO., LTD.), 80 parts by mass of molten spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, ADMATECHS COMPANY LIMITED), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK JAPAN KK), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK JAPAN KK), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0295] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg and pressed at a surface pressure of 30 kgf / cm 2 The laminate was laminated by vacuum pressing at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The measurement results are shown in Table 1.

[0296] [Example 4]

[0297] 76 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.) and a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 5 90g / eq., minimum melt viscosity: 1000Pa·s) 24 parts by mass, surface-covered titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica, alumina and dimethyl silicone (total content of silica, alumina and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass, average particle size (D50): 0.21μm, CR-63 (trade name), ISHIHARASANGYO A resin varnish was obtained by mixing 80 parts by mass of molten spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, ADMATECHS COMPANY LIMITED), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK JAPAN KK), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK JAPAN KK), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0298] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg and pressed at a surface pressure of 30 kgf / cm 2 The laminate was then vacuum pressed at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.

[0299] [Example 5]

[0300] 80 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 20 parts by mass of a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation), 80 parts by mass of a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica, alumina and dimethyl silicone (total content of silica, alumina and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass, average particle size (D50): 0.21 μm, CR-63 (trade name), ISHIHARA SANGYOKAISHA, LTD.), and 80 parts by mass of fused spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, ADMATECHS COMPANY LIMITED), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark)-161 (trade name), BYK JAPAN KK), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK JAPAN KK), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The mixing ratio (content ratio) of the surface-coated titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-coated titanium oxide: filler) in terms of volume ratio.

[0301] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg and pressed at a surface pressure of 30 kgf / cm 2 The laminate was then laminated by vacuum pressing at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) having a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.

[0302] [Comparative Example 1]

[0303] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name, K.I.CHEMICAL INDUSTRY CO., LTD.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name, Nippon Kayaku Co., Ltd.), 28 parts by mass of a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica and alumina (total content of silica and alumina: 10% by mass), titanium oxide content: 90% by mass, average particle size (D50): 0.28 μm, CR-93 (trade name), ISHIHARA SANGYO KAISHA, LTD.), 80 parts by mass of fused spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, ADMATECHS COMPANY LIMITED), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK JAPAN KK), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK JAPAN KK), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0304] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.124 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg and pressed at a surface pressure of 30 kgf / cm 2 The laminate was formed by vacuum pressing at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.1 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The measurement results are shown in Table 1.

[0305] [Comparative Example 2]

[0306] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name, K.I.CHEMICAL INDUSTRY CO., LTD.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name, Nippon Kayaku Co., Ltd.), 28 parts by mass of a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica and alumina (total content of silica and alumina: 15% by mass), titanium oxide content: 85% by mass, average particle size (D50): 0.25 μm, PFC-211 (trade name), ISHIHARA SANGYO A resin varnish was obtained by mixing 80 parts by mass of molten spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, ADMATECHS COMPANY LIMITED), 120 parts by mass of silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK JAPAN KK), 2 parts by mass of wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK JAPAN KK), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0307] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg and pressed at a surface pressure of 30 kgf / cm 2 The laminate was then laminated by vacuum pressing at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) having a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.

[0308] [Comparative Example 3]

[0309] 76 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s), 24 parts by mass of a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica and alumina (total content of silica and alumina: 15% by mass), titanium oxide content: 85% by mass, average particle size (D50): 0.25 μm, PFC-211 (trade name), ISHIHARA SANGYO A resin varnish was obtained by mixing 80 parts by mass of molten spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, ADMATECHS COMPANY LIMITED), 120 parts by mass of silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK JAPAN KK), 2 parts by mass of wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK JAPAN KK), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0310] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg and pressed at a surface pressure of 30 kgf / cm 2 The laminate was then vacuum pressed at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.

[0311] [Comparative Example 4]

[0312] A prepreg was prepared in the same manner as in Example 1 except that 80 parts by mass of surface-covered titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica, alumina and dimethyl silicone (total content of silica, alumina and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass, average particle size (D50): 0.21 μm, CR-63 (trade name), ISHIHARA SANGYOKAISHA, LTD.) was used instead of 80 parts by mass of surface-covered titanium oxide (titanium oxide particles 41% by mass, silica 57% by mass, alkyl silane 2% by mass, inorganic particles containing multiple titanium oxide particles, average particle size (D50): 4.5 μm, SUNSIL-Tin50AS (trade name), Linden Co., Ltd.). The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0313] An attempt was made to produce a metal foil-clad laminate using the obtained prepreg, but voids were generated on the entire surface of the metal foil-clad laminate, and the metal foil-clad laminate could not be produced.

[0314] [Comparative Example 5]

[0315] A prepreg was prepared in the same manner as in Example 1 except that 80 parts by mass of surface-covered titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica, alumina and dimethyl silicone (total content of silica, alumina and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass, average particle size (D50): 0.21 μm, CR-63 (trade name), ISHIHARA SANGYOKAISHA, LTD.) was used instead of 80 parts by mass of surface-covered titanium oxide (obtained by surface-treating titanium dioxide with silica and alumina, titanium oxide content: 91% by mass, average particle size (D50): 0.20 μm, R-21 (trade name), SAKAI CHEMICAL INDUSTRY CO., LTD.). The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.

[0316] An attempt was made to produce a metal foil-clad laminate using the obtained prepreg, but voids were generated on the entire surface of the metal foil-clad laminate, and the metal foil-clad laminate could not be produced.

[0317] [Evaluation Method]

[0318] (1) Relative dielectric constant (Dk) and dielectric loss tangent (Df)

[0319] The copper foils on both sides of the metal foil-clad laminates obtained in Examples and Comparative Examples were completely etched to obtain 0.1 mm thick unclad plates with all the copper foils on both sides removed. The unclad plates were cut (reduced in size) to a size of 1 mm×65 mm to obtain measurement samples.

[0320] The relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured using the measurement sample and a Network Analyzer (Agilent 8722ES (trade name), Agilent). It should be noted that the relative dielectric constant (Dk) and dielectric loss tangent (Df) were measured under a temperature of 23°C ± 1°C and a humidity of 50% RH (relative humidity) ± 5% RH.

[0321] Then, the measurement sample was dried in a dryer at 120°C for 1 hour. The dried measurement sample was subjected to a 168-hour moisture absorption treatment in a thermostatic hygrostat (FX-222P (trade name), Kusumoto Chemicals, Ltd.) at a temperature of 85°C ± 1°C and a humidity of 85% RH ± 5% RH. The relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured using a Network Analyzer (Agilent 8722ES (trade name), Agilent) for the measurement sample after the 168-hour moisture absorption treatment.

[0322] (2) Hygroscopic heat resistance evaluation

[0323] Ultra-thin copper foil (MT18FL (trade name), Mitsui Mining & Smelting Co., Ltd., thickness: 1.5 μm) with a carrier was placed on the upper and lower surfaces of the prepregs obtained in the examples and comparative examples and pressed at a surface pressure of 30 kgf / cm 2 The laminated molding is carried out by vacuum pressing for 120 minutes at a temperature of 220°C, thereby producing a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.1 mm. Then, the copper foil on both sides is completely etched to obtain an unclad plate with the copper foil on both sides completely removed. A prepreg with a thickness of 0.06 mm (GHPL-970LF (LD) (trade name), Mitsubishi Gas Chemical Co., Ltd.) is arranged on the upper and lower surfaces of the unclad plate, and an electrolytic copper foil with a thickness of 12 μm (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) is arranged on the upper and lower surfaces, and the surface pressure is 30 kgf / cm 2The laminate was formed by vacuum pressing for 120 minutes at a temperature of 220°C to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.22 mm. The obtained laminate was cut (reduced in size) to a size of 50 mm × 50 mm, and the copper foil on one side was completely removed by etching, and on the other side, half of the copper foil on the surface was removed by etching, thereby producing a sample for measurement. The obtained sample for measurement was treated for 2 hours at 121°C and 2 atmospheres of saturated water vapor using a pressure cooker tester (PC-3 type (trade name), HIRAYAMA Manufacturing Corporation), and then immersed in a solder tank at 280°C for 60 seconds to visually observe whether there was any abnormality in the appearance change. Each measurement was performed on 5 sheets each. Among these 5 sheets, when 0 to 1 sheet was observed to have an abnormal appearance, it was evaluated as "AA", when 2 to 3 sheets were observed to have an abnormal appearance, it was evaluated as "BB", and when 4 to 5 sheets were observed to have an abnormal appearance, it was evaluated as "CC". The results are shown in Table 1. It should be noted that in the sample after immersion, when swelling occurs on the surface or back of the copper foil, for example, it is judged as an abnormal appearance. In the table, "PCT 2.0h" indicates the result after 2 hours of treatment using a pressure cooker tester.

[0324] (3) Heat resistance of copper solder

[0325] Two sheets of the prepreg obtained in the examples and comparative examples were stacked, and electrolytic copper foils (3EC-M3-VLP (trade name), Mitsui Mining & Smelting Co., Ltd.) with a thickness of 12 μm were placed on the upper and lower surfaces, and the prepregs were pressed at a surface pressure of 30 kgf / cm 2 The laminated molding was carried out by vacuum pressing for 120 minutes at a temperature of 220°C, thereby producing a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.2 mm. The metal foil-clad laminate was cut (reduced in size) to a size of 50 mm × 50 mm to obtain a sample for measurement. In the same manner, all 5 samples for measurement were made. Each sample for measurement was floated in a solder tank at 300°C, so that only one side of the sample was in contact with the solder for 30 minutes. After 30 minutes, the sample was taken out of the solder tank and visually observed whether there was any change in the appearance of the side in contact with the solder in these samples. As for the results of observing the 5 samples separately, when 0 to 1 pieces of appearance abnormality were observed, it was evaluated as "AA", and when 2 to 5 pieces of appearance abnormality were observed, it was evaluated as "CC", and the results are shown in Table 1. It should be noted that in the samples taken out of the solder tank, when swelling occurs, for example, on the surface or back of the copper foil, it is judged as an appearance abnormality.

[0326] [Table 1]

[0327]

[0328] This application is based on the Japanese patent application (Japanese Patent Application No. 2022-46294) filed on March 23, 2022, the contents of which are incorporated herein by reference.

[0329] Industrial Applicability

[0330] The resin composition of this embodiment can be suitably used as a raw material for a cured product, a prepreg, a film-like underfill material, a resin sheet, a laminate, a build-up material, a non-conductive film, a metal foil-clad laminate, a printed circuit board, and a fiber-reinforced composite material, or can be suitably used in the manufacture of a semiconductor device.

Claims

1. A resin composition comprising a surface-covered titanium oxide (A) and a thermosetting compound (B), wherein the surface-covered titanium oxide (A) has a weight loss rate of 0.5 mass % or less when heated from 30° C. to 300° C. at a heating rate of 10° C. / min.

2. The resin composition according to claim 1, wherein The surface-covering titanium oxide (A) has an organic layer and / or an inorganic oxide layer on the surface of titanium oxide particles.

3. The resin composition according to claim 2, wherein The surface-covering titanium oxide (A) further has the organic layer on the surface of the inorganic oxide layer.

4. The resin composition according to claim 2, wherein The total amount of the organic layer and the inorganic oxide layer is 0.1 to 10% by mass relative to 100% by mass of the surface-covering titanium oxide (A).

5. The resin composition according to claim 2, wherein The inorganic oxide layer is one or more selected from the group consisting of a layer containing silicon dioxide, a layer containing zirconium oxide, and a layer containing aluminum oxide.

6. The resin composition according to claim 2, wherein The organic layer is a layer surface-treated with an organic silicon compound.

7. The resin composition according to claim 6, wherein The organosilicon compound includes one or more selected from the group consisting of a silane coupling agent, an organosilane, and an organopolysiloxane.

8. The resin composition according to claim 2, wherein The content of the titanium oxide in the surface-covering titanium oxide (A) is 90 to 99.9% by mass relative to 100% by mass of the surface-covering titanium oxide (A).

9. The resin composition according to claim 1, wherein The content of the surface-covering titanium oxide (A) is 50 to 500 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.

10. The resin composition according to claim 1, wherein The thermosetting compound (B) includes one or more selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, cyanate compounds, phenol compounds, alkenyl-substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having a polymerizable unsaturated group.

11. The resin composition according to claim 10, wherein The maleimide compound comprises one or more selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)-phenyl)propane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, a maleimide compound represented by the following formula (1), and a maleimide compound represented by the following formula (2), In formula (1), R 1 Each independently represents a hydrogen atom or a methyl group, and n1 is an integer from 1 to 10; In formula (2), R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, n2 is an average value, and 1 <n2≤5。 12. The resin composition according to claim 10, wherein The epoxy compound includes one or more selected from the group consisting of biphenyl aralkyl epoxy resins, naphthalene epoxy resins, and naphthyl ether epoxy resins.

13. The resin composition according to claim 10, wherein The modified polyphenylene ether compound comprises a compound represented by the following formula (3): In formula (3), X represents an aromatic group, -(YO)m- represents a polyphenylene ether portion, R1, R2 and R3 each independently represent a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group, m represents an integer from 1 to 100, n represents an integer from 1 to 6, and q represents an integer from 1 to 4.

14. The resin composition according to claim 10, wherein The cyanate compound comprises one or more selected from the group consisting of phenol novolac type cyanate compound, naphthol aralkyl type cyanate compound, naphthyl ether type cyanate compound, xylene resin type cyanate compound, bisphenol M type cyanate compound, bisphenol A type cyanate compound, diallyl bisphenol A type cyanate compound, bisphenol E type cyanate compound, bisphenol F type cyanate compound, biphenyl aralkyl type cyanate compound, and prepolymers or polymers of these cyanate compounds. 15 . The resin composition according to claim 1 , further comprising a filler (C) different from the surface-coating titanium oxide (A).

16. The resin composition according to claim 15, wherein The filler (C) includes one or more selected from the group consisting of silica, alumina, barium titanate, strontium titanate, calcium titanate, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and silicone composite powder.

17. The resin composition according to claim 15, wherein The content of the filler (C) is 50 to 300 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.

18. The resin composition according to claim 1, which is used for a printed circuit board. 19 . A prepreg comprising: a substrate, and the resin composition according to claim 1 impregnated or coated on the substrate. 20 . A resin sheet comprising the resin composition according to claim 1 .

21. A laminate comprising the prepreg according to claim 19.

22. A laminate comprising the resin sheet according to claim 20. 23 . A metal foil-clad laminate, comprising: the laminate according to claim 21 , and a metal foil disposed on one or both surfaces of the laminate. 24 . A metal foil-clad laminate, comprising: the laminate according to claim 22 , and a metal foil disposed on one or both surfaces of the laminate.

25. A printed circuit board comprising: an insulating layer, and a conductor layer disposed on one or both sides of the insulating layer, The insulating layer comprises a cured product of the resin composition according to any one of claims 1 to 18.