Tile display, unit panel set, method for manufacturing tile display, and method for maintenance of tile display

By setting a transparent substrate with anti-reflection film on the unit panel of the spliced ​​display and adjusting the color tone of the diffuse reflected light, the problem of color deviation between the unit panels is solved, and a spliced ​​display with less obvious color deviation is achieved, which improves the quality of the display and aesthetics.

CN118974803APending Publication Date: 2024-11-15AGC INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380032455.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-29
Filing Date
2023-04-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

When viewed from different angles, the color deviation of the unit panel is obvious, resulting in uneven appearance of the picture and deterioration of quality.

Method used

By setting a transparent substrate with an anti-reflection film on the display surface side of the unit panel, and adjusting the tone of the diffuse reflected light when multiple angles are incident on the light source, the a* and b* values ​​of the diffuse reflected light between adjacent panels satisfy the specific content conditions to reduce color deviation.

Benefits of technology

This realizes a splicing display with no obvious color deviation when viewed at different angles, improving the quality and aesthetics of the display.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974803A_ABST
    Figure CN118974803A_ABST
Patent Text Reader

Abstract

The present invention relates to a tiled display in which a plurality of unit panels are arranged, each of which is provided with a transparent substrate with an antireflection film on the display surface side, the transparent substrate with an antireflection film having a transparent substrate, a diffusion layer, and an antireflection film in this order toward the display surface side, and two adjacent unit panels satisfying a prescribed condition 1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a spliced ​​display, a unit panel group, a manufacturing method of the spliced ​​display and a maintenance method of the spliced ​​display. Background Art

[0002] In recent years, from the viewpoint of aesthetics, a method of providing a transparent substrate such as a cover glass in front of an image display device such as a liquid crystal display (LCD) has been used. In addition, in order to prevent external light from being reflected into the transparent substrate, a transparent substrate having an anti-reflection film (hereinafter also referred to as a transparent substrate with an anti-reflection film) is known. For example, Patent Document 1 discloses a transparent substrate having an anti-reflection film having light absorption capability and insulating properties.

[0003] In addition, in order to prevent the reflection of external light, it is also known to set a diffusion layer on the transparent substrate. The diffusion layer suppresses the reflection of external light by diffusing the incident light. As an example of a method for setting the diffusion layer, a method of laminating a film (anti-glare film) having a diffusion layer on the main surface of a transparent substrate or a panel of an image display device can be cited.

[0004] In addition, when the transparent substrate is provided with a diffusion layer, when used in an image display device, the screen when turned off may appear white due to the diffused light. Therefore, it is also considered to further provide an anti-reflection film as described above on the diffusion layer. In this way, the reflection of the incident light can be suppressed and the white color can be suppressed, so that the reflection can be appropriately controlled and the black texture of the screen when turned off can be improved.

[0005] However, in recent years, there has been a demand for larger screens for displays. If a large screen display is realized using a single display panel, problems may arise from the perspectives of mechanical strength and uneven display caused by increased electrode resistance. For this reason, it is being considered to realize a large screen by forming the display element into a panel shape and arranging multiple panels (stitching) in a tile shape as a unit panel.

[0006] For example, Patent Document 2 describes a spliced ​​display, which is characterized in that it is a spliced ​​display formed by arranging multiple unit panels with non-display areas on the peripheral portions in a tile shape, and a display sheet using organic LEDs as surface light sources is configured in a manner to cover the non-display areas located between adjacent unit panels.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2018-115105

[0010] Patent Document 2: Japanese Patent Application Publication No. 2007-192977 Summary of the invention

[0011] However, when the unit panels constituting the spliced ​​display have a transparent substrate with an anti-reflection film and an anti-glare film, the object color (diffuse reflection color) of the transparent substrate with an anti-reflection film and the anti-glare film of each unit panel may appear different depending on the angle at which the spliced ​​display is viewed. In this case, the color deviation between the unit panels becomes obvious, for example, the appearance changes to various colors when turned off, and the quality of the spliced ​​display may be greatly reduced.

[0012] Therefore, an object of the present invention is to provide a spliced ​​display with less obvious color deviation, a unit panel group used therein, a method for manufacturing the spliced ​​display, and a method for maintaining the spliced ​​display.

[0013] The inventors of the present invention have found that, when a unit panel constituting a spliced ​​display has a transparent substrate with an anti-reflection film, by focusing on the color tone (a) of diffusely reflected light when light is incident on the main surface of the display surface side of the unit panel at a predetermined angle, * and b * ), so that the diffuse reflection of light at multiple angles * and b * By satisfying prescribed conditions between adjacent unit panels, a spliced ​​display with less obvious color deviation can be obtained, thereby completing the present invention.

[0014] In addition, the inventors of the present invention have also discovered that, when the unit panels constituting the spliced ​​display are provided with an anti-glare film, by focusing on the directionality of the anti-glare property of the anti-glare film, the anti-glare index on the main surface of the display surface side of the unit panel can meet the specified conditions between adjacent unit panels, thereby obtaining a spliced ​​display with less obvious color deviation, thereby completing the present invention.

[0015] That is, the present invention relates to the following 1 to 10.

[0016] 1. A spliced ​​display, comprising a plurality of unit panels having a transparent substrate with an anti-reflection film on the display surface side,

[0017] The transparent substrate with anti-reflection film has a transparent substrate, a diffusion layer and an anti-reflection film in this order toward the display surface.

[0018] The two adjacent unit panels satisfy the condition 1 described below.

[0019] 2. The spliced ​​display according to item 1 above, wherein the haze value of the transparent substrate with the anti-reflection film is 30% or more.

[0020] 3. A unit panel set for a spliced ​​display composed of a plurality of unit panels each having a transparent substrate with an anti-reflection film on the display surface side,

[0021] The transparent substrate with anti-reflection film has a transparent substrate, a diffusion layer and an anti-reflection film in this order toward the display surface.

[0022] Two unit panels selected from the above unit panel group satisfy the condition 1 described below.

[0023] 4. The unit panel set according to item 3 above, wherein the haze value of the transparent substrate with the anti-reflection film is 30% or more.

[0024] 5. A method for manufacturing a spliced ​​display, which is a method for manufacturing a spliced ​​display formed by arranging a plurality of unit panels having a transparent substrate with an anti-reflection film on the display surface side, comprising:

[0025] For a plurality of the above-mentioned unit panels, when a light source is incident on the main surface on the display surface side at an incident angle of 45°, the diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light under a D65 light source is confirmed. * and b * ,

[0026] A combination of unit panels satisfying Condition 1 described later is selected, and the unit panels satisfying the combination are arranged so as to be adjacent to each other.

[0027] 6. A maintenance method for a spliced ​​display, which is a maintenance method for a spliced ​​display composed of a plurality of unit panels having a transparent substrate with an anti-reflection film on the display surface side, comprising:

[0028] Select the unit panel to be replaced from the unit panels that constitute the tiled display.

[0029] For at least one adjacent unit panel adjacent to the unit panel to be replaced, when a light source is incident on the main surface on the display surface side at an incident angle of 45°, the diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light is a * and b * ,

[0030] The unit panel to be replaced is replaced so that the replaced unit panel satisfies Condition 1 described later with respect to the adjacent unit panel.

[0031] 7. The spliced ​​display according to 1 or 2 above, wherein the transparent substrate with an anti-reflection film comprises an anti-glare film as the diffusion layer and the transparent substrate,

[0032] The two adjacent unit panels satisfy the condition 2 described later.

[0033] 8. A spliced ​​display, comprising a plurality of unit panels having an anti-glare film on the display surface side.

[0034] The two adjacent unit panels satisfy the condition 2 described later.

[0035] 9. A method for manufacturing a spliced ​​display, which is a method for manufacturing a spliced ​​display formed by arranging a plurality of unit panels having an anti-glare film on the display surface side, comprising:

[0036] The unit panels are arranged so that adjacent unit panels satisfy Condition 2 described later.

[0037] 10. A maintenance method for a spliced ​​display, which is a maintenance method for a spliced ​​display formed by arranging a plurality of unit panels having an anti-glare film on the display surface side, comprising:

[0038] Select the unit panel to be replaced from the unit panels constituting the spliced ​​display.

[0039] The unit panel to be replaced is replaced in such a manner that the replaced unit panel satisfies Condition 2 described later with respect to at least one adjacent unit panel adjacent to the unit panel to be replaced.

[0040] In the above 1 to 7, condition 1 is as follows.

[0041] (Condition 1)

[0042] When the light source is incident at an incident angle of 45° on the main surface of the display surface side of one of the two unit panels, the diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light is reflected under a D65 light source. * and b * Let a be the value of each angle x * and b x * , the same measurement of a on another unit panel is made * and b * Let a be the value of each angle y * and b y * When Δa of each angle * b * Below 3.0.

[0043] Δa * b * =((a x * -a y * ) 2 +(b x * -b y* ) 2 ) 1 / 2

[0044] In the above 7 to 10, condition 2 is as follows.

[0045] (Condition 2)

[0046] The L of one of the two adjacent unit panels is obtained using the following method * The angle in the direction with the maximum value is the same as the L measured for the other unit panel above. * The difference in angle between directions with the largest value is 35° or less.

[0047] (method)

[0048] On the surface parallel to the main surface of the spliced ​​display, one of the directions parallel to the common side of the two adjacent unit panels is set as the 0° direction. The light source is incident at a 45° incident angle on the main surface of the display surface side of the unit panel to be measured, and the incident direction is changed from the 0° direction to the 360° direction at 10° intervals. The L value of the diffuse reflected light at an angle of -15° relative to the specular reflected light of the incident light under the D65 light source is measured in each incident direction. * value, L * The value is the maximum incident angle L of the unit panel to be measured. * The angle in the direction where the value is maximum.

[0049] According to one embodiment of the present invention, a spliced ​​display with inconspicuous color deviation, a unit panel group used therein, a method for manufacturing the spliced ​​display, and a method for maintaining the spliced ​​display can be provided. Since the color deviation is inconspicuous, the quality and appearance of the spliced ​​display can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 It is a perspective view schematically showing a configuration example of a spliced ​​display according to the first embodiment of the present invention.

[0051] Figure 2 This is a cross-sectional view schematically showing a configuration example of a transparent substrate with an antireflection film in a unit panel.

[0052] Figure 3 is the diffuse reflection light at each angle involved in the exemplary condition 1. * and b * Schematic diagram of the assay method.

[0053] Figure 4 is an example of the diffuse reflection light at each angle related to conditions A to D. * and b *Schematic diagram of the assay method.

[0054] Figure 5 It is a perspective view schematically showing a configuration example of a spliced ​​display according to a second embodiment of the present invention.

[0055] Figure 6 This is a cross-sectional view schematically showing a configuration example of a unit panel including an anti-glare film.

[0056] Figure 7 This is a diagram schematically showing the measurement method involved in condition 2.

[0057] Figure 8 This is a diagram showing the measurement results related to Condition 2 of the spliced ​​display of Example 3.

[0058] Fig. 9 This is a diagram showing the measurement results related to Condition 2 of the spliced ​​display of Example 4.

[0059] Fig.10 This is a diagram showing the measurement results related to Condition 2 of the spliced ​​display of Example 5. DETAILED DESCRIPTION

[0060] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments, and can be arbitrarily deformed and implemented without departing from the scope of the gist of the present invention. In addition, the " to " representing a numerical range refers to the use of the meaning of including the numerical value recorded before and after it as the lower limit and upper limit.

[0061] It should be noted that in this specification, the presence of another layer, film, etc. on the main surface of a substrate such as a transparent substrate, on a layer such as a diffusion layer, on a film such as an anti-reflection film is not limited to the form in which the other layer, film, etc. is provided in contact with the above-mentioned main surface, layer or film, as long as the layer, film, etc. is provided in the upper direction thereof. For example, the presence of a diffusion layer on the main surface of a transparent substrate may mean that the diffusion layer is provided in a manner of contacting the main surface of the transparent substrate, or other arbitrary layers, films, etc. may be provided between the transparent substrate and the diffusion layer.

[0062] In this manual, unless otherwise specified, a * 、b * and L * They refer to a and b under D65 light source. * 、b * and L * .

[0063] In the following drawings, the same symbols are sometimes used to describe the components and parts having the same function, and repeated descriptions are omitted or simplified. In addition, the embodiments described in the drawings are schematic for the purpose of clearly describing the present invention, and do not necessarily accurately represent the size or ratio of actual devices, etc.

[0064] (First embodiment)

[0065] (Splicing Display)

[0066] The first embodiment of the present invention involves a spliced ​​display formed by arranging multiple unit panels having a transparent substrate with an anti-reflection film on the display surface side. The transparent substrate with the anti-reflection film has a transparent substrate, a diffusion layer and an anti-reflection film in sequence toward the display surface side, and two adjacent unit panels satisfy the following condition 1.

[0067] (Condition 1)

[0068] When the light source is incident at an incident angle of 45° on the main surface of the display surface side of one of the two unit panels, the diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light is reflected under a D65 light source. * and b * Let a be the value of each angle x * and b x * , the same measurement of a on another unit panel is made * and b * Let a be the value of each angle y * and b y * When Δa of each angle * b * Below 3.0.

[0069] Δa * b * =((a x * -a y * ) 2 +(b x * -b y * ) 2 ) 1 / 2

[0070] Figure 1 It is a perspective view schematically illustrating the spliced ​​display according to the first embodiment. Figure 1 The spliced ​​display 100 in the embodiment of the present invention comprises a unit panel 5a and a unit panel 5b arranged in a row, and is composed of two unit panels in total. The unit panels 5a and 5b are display panels having transparent substrates 1a and 1b with anti-reflection films on at least the display surface side thereof. Figure 1In the figure, the parts other than the transparent substrate with anti-reflection film constituting the display panel, such as the parts including the display elements corresponding to the image display mode (type of display), are schematically illustrated as the main body 7a, 7b forming the substantial body of the display panel. It should be noted that in this specification, the display surface side refers to the side of the spliced ​​display or unit panel that displays the image. Figures 1 to 7 In the specification, the direction toward the upper side of the paper is referred to as the display surface side. In addition, in this specification, the display surface side is sometimes referred to as the front side, and the opposite side is referred to as the back side. With respect to a spliced ​​display or a unit panel, the "front view" refers to the situation where the observer observes perpendicularly relative to the above-mentioned display surface (front), and the "oblique view" refers to the situation where the observer observes at an angle relative to the above-mentioned display surface (front).

[0071] Figure 2 It is a cross-sectional view schematically illustrating a configuration example of a transparent substrate with an antireflection film in each unit panel. Figure 2 The unit panel 5 shown has a transparent substrate 1 with an antireflection film on the front side and a main body 7 on the back side. The transparent substrate 1 with an antireflection film has a transparent substrate 10, a diffusion layer 31 and an antireflection film 30 in this order toward the front side (display surface side).

[0072] In the spliced ​​display according to the first embodiment, two adjacent unit panels satisfy the above-mentioned condition 1.

[0073] Figure 3 is the diffuse reflection light at each angle involved in the exemplary condition 1. * and b * Schematic diagram of the measurement method. In the transparent substrate 1 with an anti-reflection film arranged on the display surface side of the unit panel 5, the transparent substrate 10 has a main surface 11 and another main surface 12, and a diffusion layer 31 and an anti-reflection film 30 are formed on the one main surface 11 as the main surface on the display surface side. Light is made to be incident from a light source 50 at an incident angle of 45° to the main surface on the display surface side of the unit panel 5, that is, the one main surface 11 side of the transparent substrate 1 with an anti-reflection film. As the incident light source, a light source that emits light in the entire visible light region is used. As the light source, for example, a white light source such as a high color rendering white LED is suitable. Taking the mirror reflection light 61 of the incident light 60 as a reference (0°), the diffuse reflection lights 71, 72 and 73 are diffuse reflection lights of -15°, 15° and 25°, respectively. It should be noted that the specular reflected light 61 is set to 0°, the direction where the angle increases on the side where the incident light 60 exists is set to the + direction, and the direction where the angle increases on the side opposite to the incident light 60 is set to the - direction. The reflectance of the visible light wavelength is measured for the diffuse reflected light at each angle, and the L under the D65 light source is calculated. * 、a * and b *This measurement can be performed using, for example, CM-M6 manufactured by Konica Minolta Inc.

[0074] Here, for the main surface of the display surface side of one of the two adjacent unit panels, the diffuse reflection light at each angle is a * and b * Set a for each angle x * and b x * That is, for each main surface of the display surface side of a unit panel, the a angle of -15° is measured. x * and b x * , 15° a x * and b x * , 25° a x * and b x * . The a of -15° is measured for the other unit panel in the same manner. y * and b y * , 15° a y * and b y * , 25° a y * and b y * And, according to the -15° a x * 、b x * 、a y * and b y * , 15° a x * 、b x * 、a y * and b y * , and a of 25° x * 、b x * 、a y * and b y * The Δa calculated respectively * b *When all are below 3.0, it can be judged that condition 1 is satisfied.

[0075] Δa * b * =((a x * -a y * ) 2 +(b x * -b y * ) 2 ) 1 / 2

[0076] Two adjacent unit panels satisfying the above condition 1 means that the hue of diffusely reflected light at the same angle between the adjacent unit panels is relatively close (color difference is small). As a result, the color deviation of the spliced ​​display involved in the first embodiment is suppressed. That is, under condition 1, from the perspective of reducing the color difference of diffusely reflected light at each angle, Δa at each angle is * b * It is 3.0 or less, preferably 2.5 or less, and more preferably 2.0 or less.

[0077] In the past, when evaluating the hue of an object, it is known to evaluate the hue of reflected light by the SCE method. This is a method of evaluating the hue of the object by removing the specular reflected light from the reflected light when light is irradiated on the object and measuring only the diffuse reflected light. If the hue of the object is evaluated by the SCE method, it is possible to evaluate a hue close to that when the object is visually viewed. However, the inventors of the present invention have found that when the hues evaluated by the SCE method for two adjacent unit panels are close, although the color deviation when viewed straight on tends to become smaller, sometimes the color deviation when observed from various angles such as an inclined direction is not sufficiently suppressed. In contrast, according to the present invention, by adjusting the hue of diffuse reflected light at multiple angles for two adjacent unit panels, the color deviation when observed from various angles including an inclined direction can be suppressed.

[0078] For two adjacent unit panels, in order to obtain a spliced ​​display that meets the above requirements, as a transparent substrate with an anti-reflection film disposed on each unit panel, it is preferred to use a transparent substrate with an anti-reflection film whose angle dependence of diffuse reflected light (change in color tone caused by the angle of diffuse reflected light) is adjusted to meet the specified conditions. The specific preferred method of the transparent substrate with an anti-reflection film will be described later.

[0079] (Unit Panel)

[0080] A unit panel is a display panel that has a transparent substrate with an anti-reflection film on at least the display surface side. Multiple unit panels are arranged to form a spliced ​​display. The unit panel can be, for example, a display panel used in various displays such as a μ-LED display, a liquid crystal display (LCD display), an organic EL display (OLED display), and an electronic paper display. Its specific structure is not particularly limited depending on the type of display, etc. Figure 2 As shown, the unit panel 5 is formed by placing the transparent substrate 1 with an antireflection film on the front side of the panel-shaped main body 7 by laminating or other methods. When the transparent substrate with an antireflection film is laminated to the main body to form a unit panel, an adhesive or the like can be used as appropriate.

[0081] The type of display is not particularly limited and can be appropriately selected according to the application, etc. For example, a μ-LED display can be preferably used according to the application, etc. In the case of a μ-LED display, as described later, even when the haze of the transparent substrate with an anti-reflection film is large, it is easy to achieve high clarity.

[0082] In addition, LCD displays and OLED displays with smaller pixel pitches may also be preferably used. In order to achieve high-definition display, when the pixel pitch is smaller, the haze of the transparent substrate with an anti-reflection film may be reduced.

[0083] The size of the main surface of each unit panel is not particularly limited. For example, from the viewpoint of production cost, it is preferably 0.005 to 3 m 2 , more preferably 0.01 to 1.5 m 2 A spliced ​​display can include multiple unit panels with different main surface sizes.

[0084] The shape of the main surface of the unit panel is not particularly limited as long as it can be arranged in a tile shape, and can be appropriately selected from various shapes such as polygons and rounded rectangles according to the purpose, etc. Typically, a rectangular unit panel is preferably used as the main surface shape. In addition, the surface of the unit panel can be curved, or the panels can be arranged in a curved manner.

[0085] (Transparent substrate with anti-reflection film)

[0086] The transparent substrate with an anti-reflection film has a transparent substrate, a diffusion layer, and an anti-reflection film in this order toward the display surface side. Figure 2 In the illustrated transparent substrate 1 with an anti-reflection film, a diffusion layer 31 is formed on one main surface of the transparent substrate 10, an anti-reflection film 30 is formed on the diffusion layer 31, and the surface on the anti-reflection film side is configured as the display surface side of the unit panel. Figure 2In the example, a structure in which a diffusion layer 31 is further formed on the transparent substrate 10 is illustrated. However, as described later, the diffusion layer may be formed on the surface layer of the transparent substrate itself by a method of surface treating the transparent substrate.

[0087] When a light source is incident on one main surface of the transparent substrate with an anti-reflection film at an incident angle of 45°, the diffuse reflected light at angles of -15°, 15°, 25°, 45°, 75° and 110° relative to the specular reflected light under a D65 light source is measured. * and b * It is preferred that at least one of the following conditions A to D be satisfied.

[0088] (Condition A)

[0089] Diffuse reflected light at angles of 15°, 25° and 45° under D65 illuminant * and b * The following formulas (A1) to (A3) are satisfied.

[0090] (A1)-8≤a * ≤1

[0091] (A2)-2≤b * ≤6

[0092] (A3)b * ≤-1×a * -1

[0093] (Condition B)

[0094] Diffuse reflected light at angles of -15°, 15°, 25°, 45°, 75° and 110° under D65 light source * and b * The following formulas (B1) to (B4) are satisfied.

[0095] (B1)-6≤a * ≤2

[0096] (B2)-1≤b * ≤12

[0097] (B3)b * ≤-2a * +4

[0098] (B4)b * ≥-2a * -5

[0099] (Condition C)

[0100] Diffuse reflected light at angles of -15°, 15° and 25° under D65 light source *and b * The following formulas (C1) and (C2) are satisfied.

[0101] (C1)-5≤a * ≤-1

[0102] (C2)0≤b * ≤9

[0103] (condition D)

[0104] According to the diffuse reflection light at angles of -15°, 15° and 25° under D65 light source, a * b * The absolute value of the slope of the approximate straight line calculated by coordinates is 2 or more.

[0105] Figure 4 is a schematic illustration of the diffuse reflection light at each angle under conditions A to D. * and b * The measurement method of the diffuse reflection light at each angle under conditions A to D is shown in FIG. * and b * In the measurement, the transparent substrate with anti-reflection film is measured alone, and the diffuse reflection light at -15°, 15° and 25°, and 45°, 75° and 110° is measured. In addition, the diffuse reflection light at each angle involved in the above condition 1 is * and b * The determination method is the same. Figure 4 , diffuse reflection lights 71, 72, 73, 74, 75, and 76 are diffuse reflection lights at -15°, 15°, 25°, 45°, 75°, and 110°, respectively. It should be noted that, for example, when only confirming whether condition C is satisfied, at least diffuse reflection lights at -15°, 15°, and 25° required for confirming the condition may be measured, and the same applies to other conditions.

[0106] When measuring the transparent substrate with anti-reflection film alone, Figure 4 As shown, the reflection on the other main surface of the transparent substrate with the anti-reflection film is removed during the measurement. Figure 4 In the illustrated measurement method, for the transparent substrate 1 with an anti-reflection film, the reflection on the other main surface is removed by attaching a black tape 20 to the other main surface 12. As the black tape for removing the reflection on the other main surface, for example, "Kukiri Miel" manufactured by Tomogawa Paper Co., Ltd. can be cited, and the black tape used has a low diffuse reflectance itself and has little influence on the diffuse reflectance measurement of the surface of the transparent substrate with the anti-reflection film.

[0107] By providing a transparent substrate with an anti-reflection film with a diffusion layer and an anti-reflection film, it is possible to suppress the reflection of external light in a unit panel or a spliced ​​display, suppress the white color caused by diffuse reflected light, and improve the texture with black. On the other hand, the anti-reflection film utilizes optical interference, so the optical path length sometimes changes according to the incident angle and the emission angle of the light, and the reflected color (hue) changes in various ways. In particular, in the case of a structure with an anti-reflection film on the diffusion layer, since light is easily diffusely reflected by the diffusion layer, the brightness of the diffuse reflected light tends to become larger, and the change in hue caused by the angle tends to become more significant. For this reason, in a transparent substrate with an anti-reflection film that satisfies at least one of the above conditions A to D, the change in hue caused by the angle is suppressed by adjusting the angle dependence of the diffuse reflected light as follows.

[0108] That is, when the condition A is satisfied, the color tone changes substantially within a limited range between colorless and green depending on the angle. Therefore, various changes in the color tone depending on the angle are suppressed.

[0109] When condition B is satisfied, the hue changes roughly within a limited range between colorless and yellowish green depending on the angle. This suppresses various changes in hue depending on the angle. In addition, in this configuration, the reflected color gradually becomes brighter while maintaining yellowish green, especially from -15° to 45°, where the brightness is high. Therefore, when visually confirmed, it can be a configuration with particularly little sense of disharmony.

[0110] When condition C is satisfied, the color tone changes within a limited range of colorless or pale yellow to yellowish green depending on the angle. This suppresses various changes in the color tone depending on the angle.

[0111] When condition D is met, even if the hue changes with angle, a * The changes are small, mainly b * With such a change method, the change of color tone due to angle is likely to be limited, such as changing between colorless and a predetermined color, and various changes of color tone due to angle are suppressed. Furthermore, it becomes a structure that is less likely to cause the green to red reflected color change that humans tend to feel uncomfortable.

[0112] It should be noted that, specifically, the approximate straight line involved in condition D is a * b * The coordinates are calculated by linear approximation. * is the x-axis, b * The xy coordinate plane (a * b * In the coordinate plane, plot the diffuse reflection light at -15°, 15°, and 25° respectively. * b* The curve is obtained by least square method from these three points, y(b * ) is x(a * ) is linearly approximated to obtain an approximate straight line. For example, the approximate straight line can be obtained by linear approximation using the "Approximate Curve" function of the spreadsheet software "Microsoft Excel" (registered trademark) manufactured by Microsoft Corporation.

[0113] By using a transparent substrate with an anti-reflection film that satisfies at least one of the conditions A to D, it is easy to reduce the color difference between multiple unit panels, and the reason is explained. In order to make the angle dependence of diffusely reflected light the same between multiple transparent substrates with anti-reflection films, multiple transparent substrates with anti-reflection films having the same film structure of the anti-reflection films are prepared. However, even if multiple transparent substrates with anti-reflection films are manufactured under the same conditions, the film thickness of each dielectric layer constituting the anti-reflection film will have slight deviations, etc., so it is difficult to make the angle dependence of diffusely reflected light exactly the same. At this time, the angle dependence of the diffusely reflected light of the transparent substrate with an anti-reflection film is not properly adjusted. In the case where the color tone changes due to the angle, even if the angle dependence is slightly different, the color difference between the diffusely reflected lights at the same angle is likely to become larger. In contrast, if it is a transparent substrate with an anti-reflection film in which the change in color tone caused by angle is limited, such as satisfying at least one of conditions A to D, even if the angle dependence of the diffusely reflected light between multiple transparent substrates with anti-reflection films is not exactly the same, the color tone of the diffusely reflected light at the same angle is likely to be relatively close, and it is easy to obtain a combination of multiple transparent substrates with anti-reflection films that satisfies the above-mentioned condition 1.

[0114] It should be noted that from the viewpoint of limited change in hue due to angle, the transparent substrate with an anti-reflection film that can easily reduce color difference is not limited to satisfying any one of the conditions A to D, and the change in hue can be adjusted to a limited range in other forms. Among them, when any one of the conditions A to D is satisfied, in addition to the limited change in hue, the range of the hue change is also between colorless to a predetermined color, light yellow to yellowish green and other similar colors, which tends to be less likely to make humans feel uncomfortable, and is therefore more preferred.

[0115] In order to obtain a transparent substrate with an anti-reflection film that satisfies various conditions, it is preferred to appropriately adjust the film composition of the anti-reflection film, the light transmittance (Y) of the transparent substrate with the anti-reflection film, etc. In addition, in the case of a transparent substrate with an anti-reflection film having a high transmittance, it is difficult to rationalize using the transmittance, so it is preferred to more strictly adjust the film thickness of each layer of the anti-reflection film.

[0116] For example, when a transparent substrate with an anti-reflection film that satisfies condition A is obtained, at multiple light incident angles, the specular reflectivity relative to green light of 500nm to 550nm is preferably higher than that of blue light of 450nm to 500nm and red light of 600nm to 650nm. As a result, the specular reflection color can be maintained from black (colorless) to green at multiple light incident angles. As a result, the diffuse reflection color at multiple incident angles also tends to be maintained as colorless to green. The angular dependence of the specular reflection color can be easily predicted by using thin film simulation software. In addition, in addition to satisfying (A1) to (A3), the film thickness of each layer is adjusted to reduce the b caused by the diffuse reflection angle. * This is beneficial in reducing the reflection color deviation.

[0117] When a transparent substrate with an antireflection film satisfying condition B is obtained, the specular reflectance with respect to yellow-green light of about 500 to 600 nm is preferably higher than that with respect to blue light of 450 to 500 nm and red light of 600 to 650 nm at multiple light incident angles. As a result, the specular reflection color can be maintained from black (colorless) to yellow-green at multiple light incident angles, and as a result, the diffuse reflection color at multiple incident angles also tends to be maintained from black (colorless) to yellow-green.

[0118] For a transparent substrate with an anti-reflection film that satisfies condition C, at multiple light incident angles, the specular reflectivity with respect to green light of 500nm to 550nm is preferably higher than that with respect to blue light of 450nm to 500nm and red light of 600nm to 650nm, and the reflectivity of red light is preferably slightly higher than that of blue light. Thus, as a wavelength region with high reflectivity, green>red>blue, the specular reflection color can be maintained from black (colorless) to pale yellowish green at multiple light incident angles. As a result, the diffuse reflection color at multiple incident angles also tends to be maintained as colorless to pale yellowish green. In addition, in addition to satisfying (C1) and (C2), the film thickness of each layer is adjusted to reduce the b caused by the diffuse reflection angle. * This is beneficial in reducing the reflection color deviation.

[0119] As a method for obtaining a transparent substrate with an antireflection film that satisfies condition D, a method of adjusting the film thickness in the same manner as condition C can be cited, but the reflected color does not necessarily have to be green. For example, when the reflection of green light of 500nm to 550nm is made slightly lower than the reflection of blue light of 450nm to 500nm and red light of 600nm to 650nm, the reflected color has a tendency to be maintained in a light reddish blue to light reddish orange, which is preferred.

[0120] Furthermore, for example, by satisfying the following conditions, it is easy to obtain a transparent substrate with an antireflection film that satisfies one or more of the conditions A to D.

[0121] For example, the total thickness of the antireflection film is preferably 200 nm to 250 nm, more preferably 210 nm to 245 nm. This can suppress the angular dependence of diffuse reflection color, that is, the increase in the change in the color tone of diffuse reflection light caused by angle, and tends to easily satisfy one or more of conditions A to D.

[0122] The number of layers of the antireflection film is preferably 4 to 8, and more preferably 4 to 6. This can ensure mass productivity while suppressing an increase in the angular dependence of diffuse reflection color, and tends to make it easier to satisfy one or more of conditions A to D.

[0123] In addition, the thickness of the first high refractive index layer is the most important for the thickness of each layer, and is preferably 1 to 25 nm, and more preferably 2 to 15 nm. This can suppress the angular dependence of diffuse reflection color, that is, the increase in the change in the color tone of diffuse reflection light caused by the angle, and has a tendency to easily satisfy one or more of conditions A to D.

[0124] In the transparent substrate with an antireflection film, the haze value is preferably 30% or more, more preferably 40% or more, and further preferably 50% or more from the viewpoint of appropriately preventing reflection. From the viewpoint of improving the clarity of an image when used in an image display device, the haze value is preferably, for example, 90% or less.

[0125] In recent years, transparent substrates with anti-reflection films having a relatively high haze value as described above have been suitable for use in larger display applications. The first reason is that when the display is large, it is easier for lighting and external light to be reflected, so it is necessary to prevent reflection more appropriately. In addition, the second reason is that research is being conducted on large displays that can easily achieve high-definition displays even if the haze value is further increased, such as μ-LED displays with a large pixel pitch. However, it is known that in a transparent substrate with an anti-reflection film having a relatively high haze value, since the diffuse reflection component becomes more, as the haze increases, the change in hue of the diffuse reflected light caused by the angle and the color deviation during splicing tend to become particularly significant. In contrast, according to the present invention, even in the case of such a high haze value, a spliced ​​display in which the color deviation is appropriately suppressed can be obtained.

[0126] In addition, in the application of LCD display etc., a transparent substrate with an antireflection film having a haze value of about 0 to 30% is sometimes appropriately used. In the present invention, depending on the application etc., a haze value of 30% or less or less than 30% is not a problem.

[0127] The haze value can be adjusted by, for example, the surface shape of the diffusion layer. The haze value is measured in accordance with JIS K7136:2000 using a haze meter (HZ-V3 manufactured by SUGA Testing Instruments Co., Ltd.) or the like.

[0128] (Brightness L * )

[0129] In the transparent substrate with an anti-reflection film, according to the diffuse reflection light at each angle related to conditions A to D, * and b * The brightness L of diffuse reflected light at each angle measured in the same way * The following ranges are preferred.

[0130] -15° diffuse reflected light under D65 light source L * It is preferably 30 to 60, and more preferably 40 to 55. By making L of the diffuse reflected light at -15° * When the content is within this range, the transparent substrate with an antireflection film has appropriate light diffusivity (antiglare property) or low reflectivity, and reflection of external light can be appropriately suppressed.

[0131] 15° diffuse light under D65 light source L * It is preferably 15 to 35, and more preferably 20 to 30. By making L of the diffuse reflected light at 15° * When the content is within this range, the transparent substrate with an antireflection film has appropriate light diffusivity (antiglare property) or low reflectivity, and reflection of external light can be appropriately suppressed.

[0132] 25° diffuse light under D65 light source L * It is preferably 5 to 20, and more preferably 7 to 15. By making L * When the content is within this range, the transparent substrate with an antireflection film has appropriate light diffusivity (antiglare property) or low reflectivity, and reflection of external light can be appropriately suppressed.

[0133] (Light transmittance: Y)

[0134] The light transmittance (Y) of the transparent substrate with an anti-reflection film is preferably 20 to 90%. If the light transmittance (Y) is within the above range, the transparent substrate with an anti-reflection film has a moderate light absorption capacity, and when used as a cover glass of an image display device, it is possible to suppress the reflection of light. As a result, the contrast of the bright area of ​​the image display device is improved. The above light transmittance (Y) is more preferably 50 to 90%, and further preferably 60 to 90%. However, for example, when it is desired to maintain a high brightness of the display, it may be appropriate to use an anti-reflection film that does not have a light absorption capacity, or has a high transmittance and has a light transmittance of more than 90% as a transparent substrate with an anti-reflection film. The light transmittance (Y) in this case can be 90 to 96%, preferably 93 to 96%.

[0135] In addition, the light transmittance (Y) can be measured according to the method specified in JIS Z 8701 (1999) as described in Examples described later.

[0136] In order to make the light transmittance (Y) of the transparent substrate with an antireflection film 20 to 90%, it is preferred that, for example, a mixed oxide of at least one oxide selected from the group A consisting of Mo and W and at least one oxide selected from the group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn, and In be mainly used as the first dielectric layer of the antireflection film, and the oxidation amount of the film be adjusted. In addition, in the case of forming an antireflection film having a high transmittance and a light transmittance of 90% or more as a transparent substrate with an antireflection film, for example, at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, Mo, W, and In can be used as the first dielectric layer.

[0137] The light transmittance (Y) in the transparent substrate with an antireflection film of this embodiment can be adjusted by, for example, controlling the irradiation time, irradiation power, distance from the substrate, and amount of oxidizing gas of the oxidizing source during film formation of the first dielectric layer as a high refractive index layer in the antireflection film.

[0138] (Transparent substrate)

[0139] The refractive index of the transparent substrate having two main surfaces in this embodiment (hereinafter also referred to as the transparent substrate) is preferably 1.4 to 1.7. If the refractive index of the transparent substrate is in the above range, the reflection of the bonding surface can be fully suppressed when optical bonding is performed on a display, a touch panel, etc. The refractive index is more preferably 1.45 or more, more preferably 1.47 or more, and more preferably 1.65 or less, and more preferably 1.6 or less.

[0140] The transparent substrate preferably includes at least one of glass and resin. More preferably, the transparent substrate includes both glass and resin. By making the transparent substrate include glass, it is possible to achieve excellent strength, flatness and durability of the transparent substrate with anti-reflection film. In addition, by laminating a laminate formed by a resin substrate-diffusion layer described later on a glass substrate, it is easy to form a diffusion layer. In the transparent substrate with an anti-reflection film formed with a diffusion layer according to this method, the transparent substrate includes both glass and resin.

[0141] When the transparent substrate includes glass, the type of glass is not particularly limited, and glasses having various compositions can be used. Among them, the glass preferably includes sodium, and preferably has a composition that can be molded and strengthened by chemical strengthening treatment. As the glass, specifically, for example, aluminosilicate glass, soda-lime glass, borosilicate glass, lead glass, alkali-barium glass, aluminoborosilicate glass, etc. can be cited.

[0142] It should be noted that, in this specification, when a transparent substrate includes glass, the transparent substrate is also referred to as a glass substrate.

[0143] The thickness of the glass substrate is not particularly limited, but is preferably 5 mm or less, more preferably 3 mm or less, and further preferably 1.5 mm or less in order to effectively perform chemical strengthening when the glass is chemically strengthened.

[0144] The glass substrate is preferably a chemically strengthened glass that has been chemically strengthened. Thus, the strength of the transparent substrate with an anti-reflection film is improved. It should be noted that when the glass substrate is subjected to the anti-glare treatment described later, the chemical strengthening is preferably performed after the anti-glare treatment and before the anti-reflection film (multilayer film) is formed.

[0145] When the transparent substrate contains a resin, the type of resin is not particularly limited, and resins with various compositions can be used. Among them, the above-mentioned resin is preferably a thermoplastic resin or a thermosetting resin, for example, polyvinyl chloride resin, polyethylene resin, polypropylene resin, polystyrene resin, polyvinyl acetate resin, polyester resin, polyurethane resin, cellulose resin, acrylic resin, AS (acrylonitrile-styrene) resin, ABS (acrylonitrile-butadiene-styrene) resin, fluorine resin, thermoplastic elastomer, polyamide resin, polyimide resin, polyacetal resin, polycarbonate resin, modified polyphenylene ether resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polylactic acid resin, cyclic polyolefin resin, polyphenylene sulfide resin, etc. Among these, cellulose resin is preferred, and triacetyl cellulose resin, polycarbonate resin, polyethylene terephthalate resin can be mentioned. These resins can be used alone or in combination of two or more.

[0146] The resin particularly preferably includes at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose from the viewpoint of excellent visible light transparency and easy availability.

[0147] In addition, in this specification, when a transparent substrate contains a resin, the transparent substrate is also referred to as a resin substrate.

[0148] The shape of the resin substrate is preferably a film. When the resin substrate is a film, that is, a resin film, its thickness is not particularly limited, but is preferably 20 to 300 μm, and more preferably 30 to 130 μm.

[0149] When the transparent substrate includes both glass and resin, for example, a composite substrate in which a glass substrate and a resin substrate are laminated can be used. More specifically, the transparent substrate can be in a form in which the resin substrate is provided on the glass substrate.

[0150] (Diffusion layer)

[0151] The diffusion layer of this mode is arranged on one main surface of the transparent substrate. The diffusion layer refers to a layer having the function of diffusing specularly reflected light and reducing glare and reflection. As the diffusion layer, for example, a diffusion layer formed of a diffusion layer composition that imparts the function of diffusing specularly reflected light (anti-glare property) to the hard coating layer, a diffusion layer formed on the surface layer of the transparent substrate itself that imparts anti-glare property through surface treatment of the transparent substrate, etc. can be cited.

[0152] The diffusion layer has a concavo-convex shape on one side, or contains microparticles as scattering sources in a resin, thereby increasing the haze value through external scattering or internal scattering to impart anti-glare properties. The diffusion layer is formed of a diffusion layer composition, which is formed by, for example, dispersing a particulate substance that at least has anti-glare properties in a polymer resin dissolved as a binder. The diffusion layer can be formed by coating the above-mentioned diffusion layer composition on one main surface of a transparent substrate, for example.

[0153] Examples of the above-mentioned particulate substances having anti-glare properties include inorganic particles such as silica, clay, talc, calcium carbonate, calcium sulfate, barium sulfate, aluminum silicate, titanium oxide, synthetic zeolite, alumina, and montmorillonite, and organic particles such as styrene resins, polyurethane resins, benzoguanamine resins, silicone resins, acrylic resins, and melamine resins.

[0154] In addition, as the polymer resin of the binder of the diffusion layer, a polymer resin including, for example, polyester resin, acrylic resin, acrylic urethane resin, polyester acrylate resin, urethane acrylate resin, epoxy acrylate resin, and polyurethane resin can be used.

[0155] In this method, the diffusion layer can be directly formed on the transparent substrate, or a laminate composed of a resin substrate-diffusion layer can be prepared in advance and attached to a glass substrate, etc., so that a structure with a diffusion layer on a composite substrate of a glass substrate and a resin substrate can be obtained. The laminate is preferably a laminate in which a diffusion layer is formed on a film-like resin substrate. According to this method, it is easy to form a diffusion layer more simply.

[0156] As a laminate composed of a resin matrix-diffusion layer, specifically, for example, an anti-glare film can be cited, and more specifically, an anti-glare PET film and an anti-glare TAC film can be cited. As the anti-glare PET film, the trade names BHC-III and EHC-30a manufactured by Toyama Film Co., Ltd., the anti-glare PET film manufactured by Reiko Co., Ltd., etc. can be cited. In addition, as the anti-glare TAC film, an anti-glare TAC film (manufactured by TOPPAN TOMOEGAWAOPTICAL FILM, trade name VZ50) and the like are used.

[0157] In addition, by subjecting the transparent substrate to surface treatment, a diffusion layer can be formed on the surface of the transparent substrate itself.

[0158] For example, when a glass substrate is used, a method of performing surface treatment on the main surface of the glass to form desired projections and depressions can be used.

[0159] Specifically, the main surface of the glass substrate may be subjected to chemical treatment, such as frosting treatment. The frosting treatment may be performed by immersing the glass substrate as a treatment object in a mixed solution of hydrogen fluoride and ammonium fluoride to chemically treat the immersed surface.

[0160] In addition, in addition to chemical treatment methods such as frosting, physical treatment methods such as so-called sandblasting, in which crystalline silica powder, silicon carbide powder, etc. are blown onto the surface of the glass substrate with pressurized air, or a brush to which crystalline silica powder, silicon carbide powder, etc. is wetted with water is rubbed.

[0161] When a transparent substrate with an anti-reflection film having such a diffusion layer has a concavo-convex shape on one side of the diffusion layer, the surface has a concavo-convex shape due to the concavo-convex shape of the diffusion layer. The Sa (arithmetic mean surface roughness) of the transparent substrate with an anti-reflection film is preferably 0.05 to 0.6 μm, more preferably 0.05 to 0.55 μm. Since Sa is within this range, it is easy to suppress the reflection of the reflected image, it is preferred. For Sa, it is specified in ISO25178, for example, it can be measured using a laser microscope VK-X3000 manufactured by KEYENCE.

[0162] For the transparent substrate with an antireflection film, the developed area ratio Sdr (hereinafter also referred to as "Sdr") calculated from the surface area measured by using a laser microscope VK-X3000 manufactured by KEYENCE is preferably 0.001 to 0.4, and more preferably 0.0025 to 0.2. Sdr within this range is preferred because it is easy to suppress the reflection of the reflected image.

[0163] Sdr is defined in ISO 25178 and is represented by the following formula.

[0164] Development area ratio Sdr = {(A-B) / B}

[0165] A: Surface area (developed area) reflecting the actual concavity and convexity in the measurement area

[0166] B: The area of ​​the flat surface without unevenness in the measurement area

[0167] The Sdq (root mean square slope) of the transparent substrate with an antireflection film is preferably 0.03 to 0.50, and more preferably 0.07 to 0.49. Since Sdq is within this range, it is easy to suppress the reflection of the reflected image, so it is preferred. Sdq is specified in ISO25178 and can be measured using a laser microscope VK-X3000 manufactured by KEYENCE, for example.

[0168] The Spc (average principal curvature of the peak point of the surface) of the transparent substrate with an anti-reflection film is preferably 150 to 6000 (1 / mm). When Spc is within this range, it is easy to suppress the reflection of the reflected image, so it is preferred. Spc is specified in ISO25178 and can be measured using, for example, a laser microscope VK-X3000 manufactured by KEYENCE.

[0169] In addition, the above-mentioned Sa, Sdr, Sdq and Spc are values ​​measured on the main surface of the transparent substrate with an antireflection film on the side provided with the diffusion layer and the antireflection film.

[0170] (Barrier layer)

[0171] The transparent substrate with an anti-reflection film may have a barrier layer between the transparent substrate and the anti-reflection film. In the case where the diffusion layer is formed by a method such as bonding a laminate composed of a resin substrate-diffusion layer to a glass substrate, when the transparent substrate includes a resin substrate, a barrier layer may be provided between the diffusion layer and the anti-reflection film. By arranging the barrier layer between the resin transparent substrate and the anti-reflection film, the influence of moisture and oxygen attempting to invade the anti-reflection film from the resin substrate can be suppressed, and it has the advantages of not easily changing the optical properties, etc., so it is sometimes preferred. In addition, when the substrate includes a glass substrate in the transparent substrate, by arranging a barrier layer between the transparent substrate (glass substrate) and the anti-reflection film, it is also possible to suppress alkali metal components from diffusing into the anti-reflection film and changing the optical properties. Therefore, when the transparent substrate includes a glass substrate, a barrier layer may be provided between the transparent substrate and the anti-reflection film.

[0172] Examples of the barrier layer include metal nitride films and metal oxide films, and more specifically, SiN x Film, SiO x From the viewpoint of more effectively suppressing changes in optical properties, SiN x That is, the barrier layer preferably comprises SiN x and SiO x More preferably, the layer mainly comprises SiN x The layer is mainly composed of SiN x and SiO x At least one of the layers is composed of SiNx and SiO x At least one layer, preferably SiN x and SiO x The barrier layer is preferably a layer containing at least one of 70 mass % or more of the barrier layer. From the viewpoint of inhibiting water from entering the anti-reflection film, etc., the thickness of the barrier layer is preferably 2 nm or more, more preferably 4 nm or more, and particularly preferably 8 nm or more. On the other hand, from the viewpoint of inhibiting the increase in the reflectivity of the transparent substrate with the anti-reflection film, the thickness is preferably 50 nm or less. The barrier layer can be formed by a known film-forming method such as sputtering, vacuum evaporation, and coating.

[0173] (Anti-reflective film)

[0174] The antireflection film in the present embodiment has a function of suppressing reflection of light, and has, for example, a laminated structure in which at least two dielectric layers having mutually different refractive indices are laminated.

[0175] Figure 2 The antireflection film (multilayer film) 30 shown is a laminated structure in which two layers, a first dielectric layer 32 and a second dielectric layer 34, are laminated. By laminating the first dielectric layer 32 and the second dielectric layer 34, which have different refractive indices, the reflection of light is suppressed. For example, in Figure 2 In the embodiment, the first dielectric layer 32 is a high refractive index layer, and the second dielectric layer 34 is a low refractive index layer.

[0176] The antireflection film has a laminated structure in which at least two dielectric layers having different refractive indices are laminated, at least one of the dielectric layers is mainly composed of an oxide of Si, and at least another layer of the laminated structure is mainly composed of a mixed oxide of at least one oxide selected from the group A consisting of Mo and W and at least one oxide selected from the group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn, and In, and the content of the element of the group B contained in the mixed oxide relative to the total of the element of the group A contained in the mixed oxide and the element of the group B contained in the mixed oxide is preferably 65% ​​by mass or less. However, when it is desired to maintain high brightness of a display, in the case of appropriately using an antireflection film that does not have a light absorption capability or has a high transmittance and has a light transmittance of 90% or more as a transparent substrate with an antireflection film, at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, Mo, W, and In can be used as a layer not composed of an oxide of Si. In addition, the layer mainly composed of Si oxides may contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In within a range that has no effect on the reflectivity. By appropriately selecting the material as the oxide, an anti-reflection film with high hardness and little change in optical properties can be obtained.

[0177] exist Figure 2 In the anti-reflection film (multilayer film) 30 shown, when an anti-reflection film having a light transmittance of 90% or less as a transparent substrate with an anti-reflection film is obtained, the first dielectric layer 32 (high refractive index layer) is preferably mainly composed of at least one oxide selected from the A group consisting of Mo and W and at least one oxide selected from the B group consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In, and a mixed oxide. In addition, in the mixed oxide, the content of the elements of the B group contained in the mixed oxide relative to the total of the elements of the A group contained in the mixed oxide and the elements of the B group contained in the mixed oxide (hereinafter referred to as the B group content) is preferably 65% ​​by mass or less. Here, "mainly" means that the first dielectric layer 32 contains the largest component (based on mass), for example, it contains 70% by mass or more of the corresponding component.

[0178] If the content of group B in the first dielectric layer (A-B-O) 32 composed of a mixed oxide of at least one oxide selected from group A consisting of Mo and W and at least one oxide selected from group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In is less than 65 mass %, the yellow color of the transmitted light can be suppressed.

[0179] As at least one oxide selected from Group A, Mo or Mo and W are preferred, and as at least one oxide selected from Group B, Nb is preferred. That is, the first dielectric layer is preferably a mixed oxide of Mo and Nb or a mixed oxide of Mo, W and Nb, and more preferably a mixed oxide of Mo, W and Nb.

[0180] As described later, the second dielectric layer may also be, for example, an oxygen-deficient silicon oxide layer. Here, in the past, oxygen-deficient silicon oxide layers have a yellowish color in visible light, but if the first dielectric layer is a mixed oxide of Mo and Nb or a mixed oxide of Mo, W and Nb, the yellowing of the silicon oxide layer can be suppressed, and thus it is preferred. In addition, in order to improve reliability, the silicon oxide layer may also contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In, and each oxide may also be oxygen-deficient. Furthermore, when the second dielectric layer is formed on a diffusion layer having a higher haze as described above, i.e., a larger surface unevenness, high oxidation stability is required during film formation. If the first dielectric layer is a mixed oxide of Mo, W and Nb, it is easy to make the oxidation stability during film formation excellent, which is more preferred.

[0181] From the viewpoint of transmittance with the transparent substrate, the refractive index of the first dielectric layer 32 at a wavelength of 550 nm is preferably 1.8 to 2.5.

[0182] The extinction coefficient of the first dielectric layer 32 is preferably 0.005 to 3, and more preferably 0.04 to 0.38. If the extinction coefficient is 0.005 or more, the desired absorptivity can be achieved with an appropriate number of layers. In addition, if the extinction coefficient is 3 or less, it is easier to achieve a balance between reflective tone and transmittance.

[0183] The second dielectric layer 34 (low refractive index layer) is preferably mainly composed of Si oxide (SiO x Here, "mainly" refers to the component with the largest content (based on mass) in the second dielectric layer 34, for example, containing 70 mass% or more of the corresponding component. By making the second dielectric layer 34 (low refractive index layer) mainly composed of Si oxide (SiO x ) structure, thereby becoming a low refractive index, and the reflectivity reduction effect is improved, which is preferred. It should be noted that SiO x It can be fully oxidized silicon oxide (SiO 2 ), but from the viewpoint of improving optical reliability and scratch resistance, oxygen-deficient silicon oxide is preferred. In addition, in order to improve reliability, the silicon oxide layer may also contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In, and each oxide may also be oxygen-deficient.

[0184] Figure 2 The anti-reflection film (multilayer film) 30 shown is a laminated structure of 2 layers in total that makes the 1st dielectric layer 32 and the 2nd dielectric layer 34 laminated, but the anti-reflection film (multilayer film) in this mode is not limited to this, and can also be a laminated structure formed by the dielectric layers with different refractive indices of more than 3 layers. In this case, the refractive indices of all dielectric layers are not required to be different. For example, in the case of 3 layers of laminated structure, it can be a 3-layer laminated structure of low refractive index layer, high refractive index layer, low refractive index layer or a 3-layer laminated structure of high refractive index layer, low refractive index layer, high refractive index layer. In the case of the former, there are 2 layers of low refractive index layers that can be the same refractive index each other, and in the case of the latter, there are 2 layers of high refractive index layers that can be the same refractive index each other. In the case of 4 layers of laminated structure, it can be a 4-layer laminated structure of low refractive index layer, high refractive index layer, low refractive index layer, high refractive index layer or a 4-layer laminated structure of high refractive index layer, low refractive index layer, high refractive index layer, low refractive index layer. In this case, at least one of the two low-refractive index layers and the two high-refractive index layers may have the same refractive index.

[0185] In the case of a laminated structure in which three or more layers having different refractive indexes are laminated, the laminated structure may further include a first dielectric layer (A—B—O) 32 and a second dielectric layer (SiO x) 34. In this case, the first dielectric layer (A—B—O) 32 and the second dielectric layer (SiO x )34, and each layer is selected in such a manner as to have a three-layer stacked structure of low refractive index layer, high refractive index layer, and low refractive index layer, a three-layer stacked structure of high refractive index layer, low refractive index layer, and high refractive index layer, a four-layer stacked structure of low refractive index layer, high refractive index layer, low refractive index layer, and high refractive index layer, or a four-layer stacked structure of high refractive index layer, low refractive index layer, high refractive index layer, and low refractive index layer.

[0186] Among them, the outermost layer is preferably the second dielectric layer (SiO x )34. In order to obtain low reflectivity, if the outermost layer is the second dielectric layer (SiO x ), it is easier to make. In addition, although the reflectivity may be slightly increased, in order to improve reliability, the second dielectric layer may further contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In. In order to suppress the increase in reflectivity, the content of metals other than Si, excluding oxygen, is preferably 30 at% or less, more preferably 20 at% or less, and further preferably 15 at% or less. In addition, in the case of forming the antifouling film described later on the anti-reflection film 30, from the viewpoint of bonding related to the durability of the antifouling film, the antifouling film is preferably formed on the second dielectric layer (SiO x ) is formed on.

[0187] The first dielectric layer (A—B—O) 32 is preferably amorphous. If it is amorphous, it can be produced at a relatively low temperature and can be suitably used when the transparent substrate is made of resin and the resin is not damaged by heat.

[0188] The anti-reflection film 30 in this embodiment can be formed on the main surface of the transparent substrate using a known film forming method such as sputtering, vacuum evaporation, coating, etc. That is, the dielectric layers constituting the anti-reflection film 30 are formed on the main surface of the diffusion layer 31 according to their stacking order using a known film forming method such as sputtering, vacuum evaporation, coating, etc.

[0189] Examples of the sputtering method include magnetron sputtering, pulse sputtering, AC sputtering, and digital sputtering.

[0190] For example, magnetron sputtering is a method in which a magnet is placed on the back side of a dielectric material serving as a matrix to generate a magnetic field, causing gas ion atoms to collide with the surface of the dielectric material, escape, and sputter to form a film with a thickness of several nanometers. This method can form a continuous film of a dielectric oxide or nitride serving as the dielectric material.

[0191] In addition, for example, the digital sputtering method is different from the usual magnetron sputtering method. It is a method in which an extremely thin film of metal is first formed by sputtering, and then oxidized by irradiating oxygen plasma, or oxygen ions or oxygen free radicals, and such a process is repeated in the same chamber to form a thin film of metal oxide. In this case, the film-forming molecules are metal when attached to the substrate, so the coating is ductile compared to the case when the film is attached by the metal oxide. Therefore, it is believed that the reconfiguration of the film-forming molecules is easy to occur even with the same energy, and as a result, a dense and smooth film can be formed.

[0192] It should be noted that the above is an example of a preferred structure of the anti-reflection film, but the structure of the anti-reflection film is not limited to this. For example, when it is desired to maintain a high brightness of the display, it may be appropriate to use an anti-reflection film that has no light absorption ability or has a high transmittance and has a light transmittance of 90% or more as a transparent substrate with an anti-reflection film. In such a transparent substrate with an anti-reflection film including a high transmittance anti-reflection film, if the a of the diffusely reflected light at each angle is * and b * Within the above range, the effect of suppressing color deviation during splicing can be obtained. As the composition of the high-transmittance anti-reflection film, for example, the low-refractive index layer is the same as the second dielectric layer 34, and the high-refractive index layer has no light absorption ability or is a high-transmittance layer. As the high-refractive index layer in this case, for example, a layer mainly composed of Ti oxide (TiO x ) layer, Nb oxide (NbO x ) layer, a layer composed of Ta oxide (TaO x ) is preferably mainly composed of Ti oxide (TiO x In this case, each layer forming the antireflection film can be formed by a known film-forming method such as sputtering, vacuum evaporation, coating, etc.

[0193] When a highly transmissive antireflection film is provided, the light transmittance (Y) of the transparent substrate with an antireflection film may be, for example, 90 to 96%, and preferably 93 to 96%.

[0194] (Anti-fouling film)

[0195] From the viewpoint of protecting the outermost surface of the anti-reflection film, the transparent substrate with an anti-reflection film of this embodiment may further have an antifouling film (also called "Anti Finger Print (AFP) film") on the above-mentioned anti-reflection film. The antifouling film may be composed of, for example, a fluorinated organosilicon compound. As a fluorinated organosilicon compound, as long as it can impart antifouling properties, water repellency, and oil repellency, it can be used without particular limitation. For example, a fluorinated organosilicon compound having one or more groups selected from a polyfluoropolyether group, a polyfluoroalkylene group, and a polyfluoroalkylene group may be cited. It should be noted that a polyfluoropolyether group refers to a divalent group having a structure formed by alternating bonding of a polyfluoroalkylene group and an etheric oxygen atom.

[0196] In addition, as commercially available fluorine-containing silicone compounds having one or more groups selected from a polyfluoropolyether group, a polyfluoroalkylene group and a polyfluoroalkyl group, KP-801 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY178 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY-130 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY-185 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), OPTOOL (registered trademark) DSX and OPTOOLAES (both trade names, manufactured by DAIKIN Industries, Ltd.), etc. can be preferably used.

[0197] In the case where the transparent substrate with an anti-reflection film of this mode has an anti-fouling film, the anti-fouling film is provided on the anti-reflection film. When the anti-reflection films are provided on both sides of the two main surfaces of the transparent substrate, the anti-fouling film may be formed on the two anti-reflection films, but it may also be a configuration in which the anti-fouling film is laminated only on one main surface side. This is because the anti-fouling film can be provided at a position that may be touched by a human hand, etc., and can be selected according to its use, etc.

[0198] (Method for producing a transparent substrate with an anti-reflection film)

[0199] The method for manufacturing the transparent substrate with an anti-reflection film is not particularly limited, and for example, it can be manufactured by a method including sequentially forming a diffusion layer and an anti-reflection film on a transparent substrate. In addition, as required, it can further include forming a layer such as a barrier layer and an antifouling film.

[0200] (Composition of spliced ​​display)

[0201] The number of unit panels constituting the spliced ​​display is not particularly limited as long as it is at least two. It depends on the size of the unit panels and the desired size of the spliced ​​display, but from the perspective of large screen, the number of unit panels is preferably 2 to 1000, and more preferably 4 to 500.

[0202] The size of the spliced ​​display, that is, the area of ​​the image display surface of the spliced ​​display is not particularly limited depending on the application, etc., but is preferably 1.5 to 150 m2 from the viewpoint of enlarging the screen. 2 , more preferably 2 to 100 m 2 .

[0203] The spliced ​​display is the spliced ​​display involved in the first embodiment, and may also be the spliced ​​display involved in the second embodiment described later. In this case, in the spliced ​​display involved in the first embodiment, the transparent substrate with an anti-reflection film includes an anti-glare film as a diffusion layer and a transparent substrate, and two adjacent unit panels satisfy the condition 2 described later.

[0204] It should be noted that the transparent substrate with an anti-reflection film includes an anti-glare film as a diffusion layer and a transparent substrate, which means that the transparent substrate with an anti-reflection film includes the anti-glare film, the diffusion layer of the anti-glare film constitutes the diffusion layer of the transparent substrate with the anti-reflection film, and the resin substrate of the anti-glare film constitutes a part or all of the transparent substrate of the transparent substrate with the anti-reflection film. The anti-glare film and condition 2 in the second embodiment will be described in detail later.

[0205] (Method for manufacturing spliced ​​display)

[0206] A method for manufacturing a spliced ​​display according to a first embodiment of the present invention is a method for manufacturing a spliced ​​display formed by arranging a plurality of unit panels each having a transparent substrate with an anti-reflection film on a display surface side, comprising:

[0207] For a plurality of the above-mentioned unit panels, when a light source is incident on the main surface on the display surface side at an incident angle of 45°, a* and b* under a D65 light source of diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light are confirmed (step A11);

[0208] A combination of unit panels satisfying the above-mentioned condition 1 is selected, and the unit panels satisfying the above-mentioned combination are arranged so as to be adjacent to each other (step A12).

[0209] In the spliced ​​display, by arranging unit panels that satisfy the combination of condition 1 adjacent to each other, the color difference of diffusely reflected light at multiple angles between the unit panels is small, and color deviation is suppressed.

[0210] In step A11, for a plurality of unit panels, when a light source is incident on the main surface on the display surface side at an incident angle of 45°, the diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light under a D65 light source is confirmed. * and b * . a of diffuse reflected light at each angle * and b *The measurement method is the same as the above condition 1 involving diffuse reflected light at each angle under D65 light source a * and b * The measurement method is the same as that of the diffuse reflected light at each angle. * and b * The method may be a method of confirming the measured value measured and recorded in advance, or a method of measuring and confirming each time. Since the color tone of an object may change over time, if it is suspected that the color tone has changed due to a long time from the start of measurement, it is more preferable to re-measure and confirm the a of the diffuse reflected light at each angle. * and b * .

[0211] The plurality of unit panels to be measured are not particularly limited. For example, it is preferred to manufacture a plurality of transparent substrates with anti-reflection films that satisfy at least one of the above conditions A to D under the same conditions, and to place the plurality of transparent substrates with anti-reflection films on the display surface side as the measurement objects. Thus, it is easy to select a combination of unit panels that satisfies condition 1 from the plurality of unit panels.

[0212] In step A12, a combination of unit panels satisfying the above condition 1 is selected, and the unit panels satisfying the above combination are arranged adjacent to each other. The selection may be made based on the confirmation result of step A11.

[0213] If the number of unit panels constituting the spliced ​​display is 3 or more, in the resulting spliced ​​display, it is more preferable to arrange the unit panels in such a way that all combinations of two adjacent unit panels become combinations of unit panels that satisfy condition 1. The selection of the combination and the specific steps for arranging it are not particularly limited, and as long as the unit panel group is selected in such a way that any two unit panels selected from a plurality of unit panels satisfy condition 1, no matter how the unit panels belonging to the unit panel group are arranged, two adjacent unit panels satisfy condition 1, thereby enabling simple arrangement, which is therefore preferred.

[0214] The specific method of arranging multiple unit panels to form a spliced ​​display is not particularly limited, and a known method in spliced ​​displays can be used. For example, a method of directly connecting unit panels to each other by setting a component for connecting adjacent unit panels to each unit panel as a connecting unit, a method of indirectly connecting unit panels to each other by setting an auxiliary component on the back side of the spliced ​​display, etc. It should be noted that it is not necessary to physically connect the unit panels to each other, as long as multiple unit panels are arranged in a tiled shape, they can be regarded as a spliced ​​display.

[0215] (Unit Panel Group)

[0216] The unit panel group involved in the first embodiment of the present invention is a unit panel group used in a spliced ​​display formed by arranging multiple unit panels having a transparent substrate with an anti-reflection film on the display surface side. The above-mentioned transparent substrate with the anti-reflection film has a transparent substrate, a diffusion layer and an anti-reflection film in sequence facing the display surface side, and any two unit panels selected from the above-mentioned unit panel group satisfy the above-mentioned condition 1.

[0217] According to the unit panel group involved in the first embodiment of the present invention, when a plurality of unit panels are arranged to form a spliced ​​display, no matter how the unit panels belonging to the unit panel group are arranged, two adjacent unit panels satisfy condition 1. Thus, the spliced ​​display involved in the first embodiment of the present invention can be easily obtained.

[0218] It should be noted that the preferred embodiment of each unit panel constituting the unit panel group is the same as the unit panel used in the first embodiment. For example, the haze value of the transparent substrate with an antireflection film provided in the unit panel of the unit panel group is preferably 30% or more.

[0219] (Maintenance methods for splicing displays)

[0220] The first embodiment of the present invention involves a maintenance method for a spliced ​​display, which is a maintenance method for a spliced ​​display formed by arranging multiple unit panels having a transparent substrate with an anti-reflection film on the display surface side, comprising: selecting a unit panel to be replaced from the unit panels constituting the spliced ​​display (process B11); for at least one adjacent unit panel adjacent to the above-mentioned unit panel to be replaced, confirming a* and b* under a D65 light source of diffuse reflected light at angles of -15°, 15° and 25° relative to mirror reflected light when the light source is incident on the main surface on the display surface side at an incident angle of 45° (process B12); and replacing the above-mentioned unit panel to be replaced in a manner that the replaced unit panel satisfies the following condition 1 relative to the above-mentioned adjacent unit panel (process B13).

[0221] In step B11, a unit panel to be replaced is selected from the unit panels constituting the spliced ​​display. For example, a unit panel with a fault or a damaged unit panel can be selected as a replacement object. In addition, a unit panel that operates normally can be selected as a replacement object. For example, a specific selection criterion is set for the purpose of preventing faults, and a unit panel that meets the criterion is selected as a replacement object. The unit panel to be replaced can be one or more.

[0222] In step B12, for at least one adjacent unit panel adjacent to the unit panel to be replaced, when a light source is incident on the main surface on the display surface side at an incident angle of 45°, a* and b* of diffuse reflection light at angles of -15°, 15°, and 25° relative to the mirror reflection light under the D65 light source are confirmed. In step B12, the object to be confirmed is a* of diffuse reflection light at each angle of the adjacent unit panel. * and b * , except for this, the process is the same as the above-mentioned step A11. As these confirmation methods, there may be a method of confirming information (measured values, etc.) measured and recorded in advance, or a method of measuring and confirming each time.

[0223] In step B13, the unit panel to be replaced is replaced in such a manner that the replaced unit panel satisfies the following condition 1 relative to the adjacent unit panel. The replacement here means replacing only the transparent substrate with an anti-reflection film in the unit panel, in addition to replacing all unit panels with other unit panels, and also includes replacing a part of the unit panel. It is preferred that appropriate unit panels and transparent substrates with anti-reflection films are selected based on the confirmation results in step B12.

[0224] According to the maintenance method of the tiled display according to the first embodiment of the present invention, when a part of the unit panel in the tiled display is replaced, the color deviation of the tiled display after the replacement can be suppressed.

[0225] It should be noted that when there are multiple adjacent unit panels relative to a unit panel to be replaced, if at least one of the adjacent unit panels is subjected to step B12 and step B13, the color difference between the adjacent unit panel and the replaced unit panel is suppressed. If all adjacent unit panels are subjected to step B12 and step B13, the color difference between all adjacent unit panels and the replaced unit panel is suppressed, which is more preferred.

[0226] (Second embodiment)

[0227] (Splicing Display)

[0228] A spliced ​​display according to a second embodiment of the present invention is a spliced ​​display formed by arranging a plurality of unit panels each having an anti-glare film on a display surface side, wherein two adjacent unit panels satisfy the following condition 2.

[0229] (Condition 2)

[0230] The L of one of the two adjacent unit panels is obtained using the following method * The angle in the direction with the maximum value is the same as the L measured for the other unit panel above. * The difference in angle between directions with the largest value is 35° or less.

[0231] (method)

[0232] On the surface parallel to the main surface of the spliced ​​display, one of the directions parallel to the common side of the two adjacent unit panels is set as the 0° direction. The light source is incident at a 45° incident angle on the main surface of the display surface side of the unit panel to be measured, and the incident direction is changed from the 0° direction to the 360° direction at 10° intervals. The L value of the diffuse reflected light at an angle of -15° relative to the specular reflected light of the incident light under the D65 light source is measured in each incident direction. * value, L * The value is the maximum incident angle L of the unit panel to be measured. * The angle in the direction where the value is maximum.

[0233] Figure 5 It is a perspective view schematically illustrating a spliced ​​display according to the second embodiment. Figure 5 The spliced ​​display 200 in the embodiment is composed of two unit panels, namely, a unit panel 205a and a unit panel 205b. The unit panels 205a and 205b are display panels having anti-glare films 201a and 201b at least on their display surface sides. Figure 5 In the figure, the parts other than the anti-glare film constituting the display panel, such as the parts including the display elements corresponding to the image display mode (type of display), are schematically illustrated as the main body 207a, 207b forming the substantial body of the display panel.

[0234] Figure 6 It is a cross-sectional view schematically illustrating a configuration example of the anti-glare film in each unit panel. Figure 6 The unit panel 205 shown includes an anti-glare film 201 on the front side and a main body 207 on the back side. The anti-glare film 201 includes a resin base 210 and a diffusion layer 231 formed on the resin base 210.

[0235] In the spliced ​​display according to the second embodiment, two adjacent unit panels satisfy the above-mentioned condition 2.

[0236] Here, condition 2 involves L * The angle in the direction with the maximum value is measured by the above-mentioned method, and more specifically, as follows.

[0237] Figure 7 The L is measured for two adjacent unit panels 205a and 205b in the spliced ​​display 200. * More specifically, Figure 7 The L of the diffusely reflected light at -15° when the incident direction is 0° for the unit panel 205b is shown schematically.* Value graph.

[0238] In the measurement, first, on a surface parallel to the main surface of the spliced ​​display, one of the directions parallel to the sides shared by two adjacent unit panels is set as the 0° direction. Figure 7 When looking at the spliced ​​display, the direction parallel to the side S shared by the unit panel 205a and the unit panel 205b is Figure 7 The direction in front is set as the 0° direction D1. It is arbitrary which direction of the directions parallel to the edges shared by two adjacent unit panels is set as the 0° direction. When two adjacent unit panels do not share a straight edge, any direction on the main surface of the spliced ​​display is set as the 0° direction. In addition, directions of 0° to 360° are defined as directions in which the angle increases in the clockwise direction when looking directly at the spliced ​​display. Among them, the 0° direction and the 360° direction are the same direction. The light source is made to be incident on the main surface of the display surface side of the unit panel as the measurement object at an incident angle of 45°, and the incident direction is changed from the 0° direction to the 360° direction at intervals of 10°, for example, as Figure 7 As shown in FIG. 1 , when the trajectory of incident light 80 and diffusely reflected light 81 is projected onto a surface parallel to the main surface of the spliced ​​display, the light on the projection trajectory P is traveling in a 0° direction, which can be defined as the light source being incident in a 0° direction. Furthermore, for each incident direction, the L value of diffusely reflected light at an angle of -15° relative to the specularly reflected light of the incident light under the D65 light source is measured. * That is, when the incident direction is 0°, the above L * Value, the above L at 10° direction * Value, ... for the above L in the 360° direction * The above L values ​​are measured in 36 directions for a unit panel. * And, L in 36 directions * The value is the maximum incident angle L of the unit panel to be measured. * The angle of the direction in which the value is the largest. Here, the diffuse reflection light at an angle of -15° relative to the mirror reflection light is the same as the diffuse reflection light at -15° involved in condition 1 in the first embodiment described above. The measurement related to condition 2 can be performed using, for example, CM-M6 manufactured by Konica Minolta. The light source and measurement conditions used in the measurement can be the same as the light source and measurement conditions used in the measurement involved in condition 1.

[0239] The above measurements were performed on two adjacent unit panels respectively, and the L * The angles of the directions with the largest values ​​are used to determine whether condition 2 is satisfied. *The difference between the angles in the directions with the largest value is used to evaluate the actual closeness of the angles in the two directions. That is, the difference is 0° to 180°. For example, for two unit panels, if L * The angles of the directions with the largest values ​​are 10° and 350°, and their difference is 20°.

[0240] The above L is different according to the direction on the measured surface. * The difference in value means that the degree of light diffusion varies depending on the direction on the measured surface, that is, depending on the direction from which the measured surface is viewed. * A large value means that the diffuse reflectivity of the anti-glare film is high and the light diffusivity is higher. In addition, in the anti-glare film, there is usually a large diffuse reflectivity in the width direction (TD) of the diffuse reflectivity in the direction parallel to the liquid flow direction (MD) during manufacturing, and the diffuse reflectivity in one of the directions parallel to MD on the surface of the anti-glare film is approximately the largest, and the diffuse reflectivity in one of the directions parallel to TD is approximately the smallest. Therefore, the two adjacent unit panels satisfying the above condition 2 means that the directions of the anti-glare films of the two unit panels during manufacturing are also consistent with each other on the main surface of the spliced ​​display, or are configured with a small inclination. In other words, it means that the orientations of the anti-glare films of the adjacent unit panels on the spliced ​​display are relatively consistent. It is therefore believed that the deviation in the way the light diffusivity of the adjacent unit panels changes when the spliced ​​display is observed from various directions can be suppressed, so that the color deviation between the unit panels is not obvious. It should be noted that the SCE method is known as described above, and it is known that the color tone of an object can be evaluated by measuring diffuse reflected light. Therefore, it can be considered that in the second embodiment, the L of the diffuse reflected light between the unit panels is suppressed. * deviation, which helps to suppress color deviation.

[0241] From the viewpoint of more appropriately obtaining the above-mentioned effect, in condition 2, L * The difference between the angles of the directions with the largest values ​​is 35° or less, preferably 30° or less, and more preferably 25° or less. * The difference between the angles of the directions with the maximum values ​​may be 0°.

[0242] The method for obtaining a spliced ​​display satisfying condition 2 is not particularly limited, and for example, a method of preparing a plurality of unit panels obtained by configuring an anti-glare film (laminating) in a manner parallel to any direction of the anti-glare film (for example, one direction in the direction parallel to the MD) and any direction of the main surface of the unit panel (for example, the long side direction), and arranging them, etc. That is, it is preferred that the directions of the anti-glare films of the adjacent unit panels during manufacture are consistent with each other even on the main surface of the spliced ​​display, or the unit panels are prepared and arranged in a manner with a small inclination. It should be noted that parallel here means that the inclination angle relative to the reference line is, for example, within 30°.

[0243] The L values ​​of two adjacent unit panels measured at 10° intervals according to the above method are * The difference between the maximum values ​​of the values ​​is preferably less than 3, more preferably less than 2, and further preferably less than 1. When the difference between the maximum values ​​of two adjacent unit panels is small, it can be considered that the degree of the anti-glare properties in the two adjacent unit panels is the same. Thus, not only the deviation of the anti-glare properties between the unit panels caused by the difference (directivity) of the diffuse reflection in the direction on the anti-glare film can be suppressed, but also the deviation caused by the size of the anti-glare properties of the unit panels can be suppressed, and the color deviation can be more appropriately suppressed. For example, in a plurality of transparent substrates with anti-glare films obtained from the anti-glare films manufactured under the same manufacturing conditions and the unit panels having the same, usually, the difference between the maximum values ​​is within the above range.

[0244] (Unit Panel)

[0245] The unit panel is a display panel having an anti-glare film at least on its display surface side. The unit panel in the second embodiment is the same as the unit panel in the first embodiment except that the anti-glare film is provided on its display surface side instead of the transparent substrate with an anti-reflection film. It should be noted that, as described in detail later, the anti-glare film may also be a transparent substrate with an anti-reflection film further having an anti-reflection film on the anti-glare film. In addition, the transparent substrate with an anti-glare film in which the anti-glare film is bonded to the transparent substrate may be provided on the display surface side of the unit panel.

[0246] (Anti-glare film)

[0247] The anti-glare film has a resin matrix and a diffusion layer formed on the resin matrix. The diffusion layer is formed by forming a layer with a concave-convex shape on the surface or coating a resin mixed with microparticles, thereby increasing the haze and imparting anti-glare properties. As described above, in the anti-glare film, the diffuse reflectance in the liquid flow direction (MD) during manufacturing is usually greater than the diffuse reflectance in the width direction (TD), so the L in one direction parallel to the MD on the surface of the anti-glare film is greater than the L in the width direction (TD). * The value is roughly the largest, and L in one direction parallel to TD * The value tends to be approximately the smallest. It can be considered that this L * The difference in the values ​​is caused by the difference in tension between MD and TD when the anti-glare liquid is applied to the resin substrate of the anti-glare film in a roll-to-roll manner. Therefore, as the anti-glare film used in the second embodiment, an anti-glare film in which the anti-glare liquid is wet-coated on the resin substrate of the anti-glare film in a roll-to-roll manner can be appropriately used. * The anti-glare film is not limited to the above-mentioned form if the values ​​have the same directivity.

[0248] The material of the resin matrix of the anti-glare film is not particularly limited, and for example, a thermoplastic resin or a thermosetting resin can be used. Examples of thermoplastic resins or thermosetting resins include polyvinyl chloride resins, polyethylene resins, polypropylene resins, polystyrene resins, polyvinyl acetate resins, polyester resins, polyurethane resins, cellulose resins, acrylic resins, AS (acrylonitrile-styrene) resins, ABS (acrylonitrile-butadiene-styrene) resins, fluorine resins, thermoplastic elastomers, polyamide resins, polyimide resins, polyacetal resins, polycarbonate resins, modified polyphenylene ether resins, polyethylene terephthalate resins, polybutylene terephthalate resins, polylactic acid resins, cyclic polyolefin resins, polyphenylene sulfide resins, etc. Among them, cellulose resins are preferred, and triacetyl cellulose resins, polycarbonate resins, and polyethylene terephthalate resins are more preferred.

[0249] The thickness of the resin substrate is not particularly limited, but is preferably 10 μm or more, more preferably 20 μm or more, from the viewpoint of productivity, and preferably 100 μm or less, more preferably 80 μm or less, from the viewpoint of design.

[0250] The diffusion layer is obtained by, for example, applying a composition (diffusion layer composition) in which a particulate substance having at least antiglare properties is dispersed in a solution in which a polymer resin serving as a binder is dissolved, to a resin base and drying the composition.

[0251] Examples of the above-mentioned granular substances having anti-glare properties include inorganic particles such as silica, clay, talc, calcium carbonate, calcium sulfate, barium sulfate, aluminum silicate, titanium oxide, synthetic zeolite, alumina, and montmorillonite, and organic particles composed of styrene resins, polyurethane resins, benzoguanamine resins, silicone resins, acrylic resins, and the like.

[0252] In addition, as the polymer resin of the adhesive, polyester resin, acrylic resin, acrylic urethane resin, polyester acrylate resin, urethane acrylate resin, epoxy acrylate resin, polyurethane resin and the like can be used. From the viewpoint of film hardness, the polymer resin of the adhesive is preferably acrylic resin.

[0253] As the anti-glare film, a commercial product may also be used. Examples of commercially available anti-glare films include anti-glare PET films and anti-glare TAC films. Examples of anti-glare PET films include BHC-III and EHC-30a manufactured by Toyama Film Co., Ltd., and anti-glare PET films manufactured by Reiko Co., Ltd. In addition, as the anti-glare TAC film, an anti-glare TAC film (manufactured by TOPPAN TOMOEGAWAOPTICAL FILM, trade name VZ50) and the like may be used.

[0254] When the anti-glare film has a concavo-convex shape on one side of the diffusion layer, the surface has a concavo-convex shape due to the concavo-convex shape of the diffusion layer. For example, at least one of Sa, Sdr, Sdq and Spc of the anti-glare film in the second embodiment may be the same as the preferred Sa, Sdr, Sdq and Spc of the transparent substrate with anti-reflection film in the first embodiment. In addition, the haze of the anti-glare film in the second embodiment may also be the same as the preferred haze of the transparent substrate with anti-reflection film in the first embodiment.

[0255] The shape of the anti-glare film is usually the same as the shape of the main surface of one side of the anti-glare film bonded to the unit panel or the transparent substrate. However, in the case where a part of the main surface bonded with the anti-glare film is not flat or the part having a specific function such as a camera is not given anti-glare properties, the shape of the anti-glare film may be processed in such a way that the anti-glare film is not bonded to a specific area of ​​the main surface. In addition, for the same reason, a part of the anti-glare film may be provided without a diffusion layer.

[0256] (Adhesive)

[0257] In order to bond the anti-glare film to the unit panel or the transparent substrate, it is preferred to use an adhesive as necessary.

[0258] As the adhesive, acrylic adhesive, silicone adhesive, polyurethane adhesive, etc. can be cited. From the viewpoint of durability, the adhesive is preferably an acrylic adhesive. The adhesive can be applied on the surface of the diffusion layer without an anti-glare film, or can also be applied on the surface of the anti-glare film attached to a transparent substrate, but from the viewpoint of durability, it is preferred to apply the adhesive on the anti-glare film. In addition, an adhesive pre-formed into a sheet or the like can also be used. In addition, in the case where the resin matrix of the anti-glare film has self-adsorption, etc., the anti-glare film can also be attached to the transparent substrate without using an adhesive. It should be noted that an anti-glare film pre-equipped with an adhesive can also be used in commercial products, etc.

[0259] (Transparent substrate)

[0260] The anti-glare film includes a resin matrix, but as required, the anti-glare film may be laminated on a transparent matrix different from the resin matrix constituting the anti-glare film to form a transparent matrix with an anti-glare film, and the transparent matrix may be arranged on the display surface side of the unit panel. When the transparent matrix with an anti-glare film is arranged on the display surface side of the unit panel, the preferred mode of the transparent matrix in the transparent matrix with an anti-glare film is the same as the preferred mode of the transparent matrix in the first embodiment.

[0261] (Barrier layer)

[0262] When the anti-glare film further includes an anti-reflection film, the anti-glare film preferably includes a barrier layer between the diffusion layer and the anti-reflection film. Preferred aspects of the barrier layer in the second embodiment are the same as those of the barrier layer in the first embodiment.

[0263] (Anti-reflective film)

[0264] The anti-glare film may also include an anti-reflection film. In this case, the anti-glare film with the anti-reflection film may also be regarded as a transparent substrate with an anti-reflection film having a diffusion layer and an anti-reflection film on a transparent substrate (resin substrate in the anti-glare film). In the second embodiment, the anti-glare film may be arranged on the display surface side of the unit panel by arranging such a transparent substrate with an anti-reflection film on the display surface side of the unit panel. The anti-reflection film is preferably arranged on the diffusion layer, that is, arranged on the side opposite to the transparent substrate when viewed from the diffusion layer. It should be noted that, as described above, other layers such as a barrier layer may also be provided between the diffusion layer and the anti-reflection film, and the diffusion layer and the anti-reflection film may not be in contact with each other. The specific composition of the anti-reflection film is not particularly limited as long as it is a composition that can suppress the reflection of light, and for example, it may be the same anti-reflection film as the anti-reflection film exemplified in the first embodiment.

[0265] (Anti-fouling film)

[0266] From the viewpoint of protecting the outermost surface, the transparent substrate with an anti-glare film may also have an anti-fouling film. The anti-fouling film is preferably arranged on the outermost surface on the side opposite to the transparent substrate when viewed from the diffusion layer of the transparent substrate with an anti-glare film. The specific material and preferred mode of the anti-fouling film in the second embodiment are the same as those of the anti-fouling film in the first embodiment.

[0267] (Composition of spliced ​​display)

[0268] The number of unit panels constituting the tiled display in the second embodiment and the size of the tiled display are not particularly limited, and preferred aspects thereof are the same as those of the tiled display in the first embodiment.

[0269] The spliced ​​display is the spliced ​​display according to the second embodiment and may also be the spliced ​​display according to the first embodiment. In this case, the spliced ​​display according to the second embodiment has a transparent substrate with an anti-reflection film, and two adjacent unit panels satisfy the above-mentioned condition 1.

[0270] (Method for manufacturing spliced ​​display)

[0271] The second embodiment of the present invention relates to a method for manufacturing a spliced ​​display comprising arranging a plurality of unit panels having anti-glare films on the display surface side, and includes arranging the unit panels in such a manner that adjacent unit panels satisfy the above-mentioned condition 2 (step A21).

[0272] In the spliced ​​display, adjacent unit panels are arranged so as to satisfy condition 2, thereby suppressing the variation in the degree of anti-glare properties between the unit panels and suppressing color deviation.

[0273] In step A21, as a method of arranging unit panels in such a manner that adjacent unit panels satisfy condition 2, for example, a method of preparing a plurality of unit panels in which an anti-glare film is arranged (laminated) in such a manner that any direction on the anti-glare film (for example, one direction in parallel with the MD) is parallel to any direction of the main surface of the unit panel (for example, the long side direction), and arranging them, etc. That is, it is preferred to prepare and arrange the unit panels in such a manner that the directions of the anti-glare films possessed by the adjacent unit panels during manufacturing are consistent with each other even on the main surface of the spliced ​​display, or in such a manner that the inclination is small. Alternatively, it is preliminarily confirmed that the L of -15° in multiple directions on the unit panel * value, or when the L * The unit panels are arranged in the direction of the maximum value according to the confirmation result so that the adjacent unit panels can satisfy condition 2. These confirmation methods may be a method of confirming information (measured values, etc.) measured and recorded in advance or a method of measuring and confirming each time.

[0274] If the number of unit panels constituting the spliced ​​display is three or more, in the resulting spliced ​​display, the unit panels are preferably arranged so that all combinations of two adjacent unit panels satisfy condition 2.

[0275] The specific method of arranging a plurality of unit panels to form a spliced ​​display is not particularly limited, and a known method in spliced ​​displays may be used. For example, the spliced ​​display may be formed using the method exemplified in the method for manufacturing a spliced ​​display according to the first embodiment.

[0276] (Maintenance methods for splicing displays)

[0277] The second embodiment of the present invention involves a maintenance method for a spliced ​​display, which is a maintenance method for a spliced ​​display formed by arranging multiple unit panels with anti-glare films on the display surface side, comprising: selecting a unit panel to be replaced from the unit panels constituting the spliced ​​display (process B21); and replacing the unit panel to be replaced in a manner that the replaced unit panel satisfies the above-mentioned condition 2 relative to at least one adjacent unit panel adjacent to the unit panel to be replaced (process B22).

[0278] In step B21, a unit panel to be replaced is selected from the unit panels constituting the spliced ​​display. Step B21 is the same as step B11 in the spliced ​​display maintenance method according to the first embodiment.

[0279] In step B22, the unit panel to be replaced is replaced in such a way that the replaced unit panel satisfies the above-mentioned condition 2 relative to at least one adjacent unit panel adjacent to the unit panel to be replaced. The replacement here refers to replacing all unit panels with other unit panels, and also includes replacing only a part of the unit panel such as the anti-glare film in the unit panel. As a specific method for replacing the unit panel to be replaced in a manner that satisfies the above-mentioned condition 2, for the unit panels and adjacent unit panels that can be used in the replacement, the bonding direction of the anti-glare film possessed by each unit panel is confirmed, and the unit panel is replaced based on the confirmation result. Alternatively, the -15° L in multiple directions on the unit panel may be confirmed in advance. * value or the L * The unit panel is replaced according to the confirmation result. As these confirmation methods, there may be a method of confirming information (measured values, etc.) measured and recorded in advance, or a method of measuring and confirming each time.

[0280] According to the maintenance method of a tiled display according to the second embodiment of the present invention, when a part of a unit panel in the tiled display is replaced, it is possible to suppress color deviation of the tiled display after the replacement.

[0281] It should be noted that when there are multiple adjacent unit panels relative to a unit panel to be replaced, if step B22 is performed on at least one of the adjacent unit panels, the color difference between the adjacent unit panel and the replaced unit panel can be suppressed. If step B22 is performed on all adjacent unit panels, the color difference between all adjacent unit panels and the replaced unit panel can be suppressed, which is more preferred.

[0282] Example

[0283] The present invention is specifically described below with reference to examples, but the present invention is not limited thereto.

[0284] (Example 1, Example 2)

[0285] The following Examples 1 and 2 are examples related to the above-mentioned first embodiment.

[0286] Transparent substrates 1 to 3 with anti-reflection films and unit panels 1 to 3 having the same were prepared, and spliced ​​displays obtained by arranging them were evaluated. The spliced ​​display obtained by combining unit panels 1 and 2 (the spliced ​​display of Example 1) corresponds to the embodiment, and the spliced ​​display obtained by combining unit panels 1 and 3 (the spliced ​​display of Example 2) corresponds to the comparative example.

[0287] (evaluate)

[0288] (a of diffuse reflected light at each angle * b * L* )

[0289] The diffuse reflection light a at each angle was measured for the main surface of the display surface side of the unit panel or the transparent substrate with an anti-reflection film by the following method: * b * L * In the measurement of the main surface on the display side of the unit panel, the measurement was performed with the screen turned off. In the measurement of the transparent substrate with anti-reflection film alone, a black tape (Kukiri Miel, manufactured by Tomogawa Paper Co., Ltd.) was attached to the main surface (the other main surface) of the transparent substrate with anti-reflection film that did not have a diffusion layer and an anti-reflection film to remove the reflection on the other main surface.

[0290] The light source is incident at an incident angle of 45° on the main surface (one main surface) of the transparent substrate with the anti-reflection film having the diffusion layer and the anti-reflection film. The reflectance of the visible light wavelength is measured for each diffuse reflection light at an angle of -15°, 15° and 25° relative to the mirror reflection light, and the a under the D65 light source is calculated. * , b * and L * (Diffuse reflection color) The measurement was performed using CM-M6 manufactured by Konica Minolta Inc.

[0291] (SCI, SCE)

[0292] The reflectance color (L) of the main surface of the display surface side of the unit panel or the transparent substrate with an anti-reflection film was measured by the SCI method and the SCE method. * 、a * and b * ). All measurements were performed using a spectrophotometer (manufactured by Konica Minolta, trade name: CM-26d) in accordance with the method specified in JIS Z 8722 (2009). It should be noted that in the SCE method, specular reflection light is removed from reflected light when light is irradiated on an object, and only diffuse reflection light is measured, whereas in the SCI method, all reflected light including specular reflection light is measured.

[0293] In the measurement of the main surface of the display surface side of the unit panel, the measurement was performed after the screen was turned off. In addition, in the measurement of the transparent substrate with anti-reflection film alone, black tape (Kukiri Miel, manufactured by Tomogawa Paper Co., Ltd.) was attached to the main surface (the other main surface) of the transparent substrate with anti-reflection film that did not have a diffusion layer and an anti-reflection film to remove the reflection on the other main surface.

[0294] (Haze)

[0295] The haze value (transmission haze) of the transparent substrate with an antireflection film was measured in accordance with JIS K 7136:2000 using a haze meter (HZ-V3 manufactured by SUGA Testing Instruments Co., Ltd.).

[0296] (Light transmittance: Y)

[0297] In a transparent substrate with an anti-reflection film, the light transmittance (Y) of the outermost surface of the anti-reflection film is measured according to the method specified in JIS Z8701 (1999). It should be noted that in this specification, the light transmittance (Y) of the outermost surface of the anti-reflection film is set as the light transmittance (Y) in the transparent substrate with the anti-reflection film. Specifically, of the two main surfaces of the transparent substrate, a black tape is attached to the main surface other than the anti-reflection film side, so that the spectral transmittance is measured by a spectrophotometer (manufactured by Shimadzu Corporation, trade name: SolidSpec-3700) after removing the back reflection, and the light transmittance (stimulation value Y specified in JIS Z 8701 (1999)) is calculated.

[0298] (Color deviation evaluation)

[0299] Prepare 96 transparent substrates with anti-reflection films made under the same conditions as the transparent substrate 1 with anti-reflection films in the unit panel 1. Specifically, prepare 96 transparent substrates with anti-reflection films made under the conditions in the transparent substrate 1 with anti-reflection films and slightly change the film thickness of each layer from the conditions. Then, after pasting black tape (made by Tomogawa Paper Co., Ltd., Kukiri Miel) on the main surface (the other main surface) without the diffusion layer and the anti-reflection film, they are arranged (spliced) in a vertical 12 × horizontal 8 without gaps. The color deviation of the spliced ​​transparent substrate with anti-reflection film is visually evaluated according to the following criteria and divided into two levels of "good" and "unacceptable". Then, prepare a "good" and "unacceptable" sample without black tape on the back, use the "good" sample as the transparent substrate 2 with anti-reflection film for the unit panel 2, and use the "unacceptable" sample as the transparent substrate 3 with anti-reflection film for the unit panel 3. The transparent substrates 1 to 3 with anti-reflection films were bonded to the display surface of a self-luminous OLED display (Pixel 6Pro manufactured by Google) with a transparent adhesive so that the side with the anti-reflection films formed thereon became the display surface side, thereby forming unit panels 1 to 3. For each unit panel, SCI, SCE, and diffuse reflection color at each angle were obtained.

[0300] Good: When white LED lighting is reflected on the main surface (one main surface) of a transparent substrate with an anti-reflection film on one side having a diffusion layer and an anti-reflection film and observed from various angles, the white lighting reflected on the transparent substrate with the anti-reflection film appears to be a color close to achromatic, which is the result of the color difference between the substrates being not obvious.

[0301] No: When white LED lighting is reflected on the main surface (one main surface) of the transparent substrate with an anti-reflection film on the side having the diffusion layer and the anti-reflection film and observed from various angles, the result is a clear color difference from the surroundings.

[0302] Next, the spliced ​​display of Example 1 consisting of two unit panels was formed by arranging unit panel 1 and unit panel 2. In addition, the spliced ​​display of Example 2 consisting of two unit panels was formed by arranging unit panel 1 and unit panel 3. For each spliced ​​display, the color deviation in normal view and oblique view was evaluated according to the following criteria.

[0303] “None”: When visually observing the spliced ​​display, no difference in color tone (reflected color) between unit panels is detected.

[0304] “Yes”: When visually viewing the spliced ​​display, the difference in hue (reflected color) between the unit panels is noticeable, and the color deviation is obvious.

[0305] In addition, the diffuse reflection light a of the unit panel 1 at each angle is * and b * Set to a x * and b x * , calculate the diffuse reflection light a at each angle of each example * and b * Set to a y * and b y * Δa of each angle when * b * . Calculate Δa similarly for SCI and SCE * b * .

[0306] (Transparent substrate 1 with anti-reflection film)

[0307] According to the following method, an anti-reflection film was formed on an anti-glare PET film having a diffusion layer formed on one main surface of a transparent substrate to produce a transparent substrate with an anti-reflection film. It should be noted that the transparent substrate was a resin substrate as described later.

[0308] (transparent substrate, diffusion layer)

[0309] An anti-glare PET film of 50 mm in length×50 mm in width×0.1 mm in thickness (manufactured by Reiko Co., Ltd., Sa: 0.259 μm, Sdr: 0.0620, Sdq: 0.361, Spc: 1703 (1 / mm), haze value: 60%) was used.

[0310] (Film formation of barrier layer)

[0311] Next, a SiN layer was formed as a barrier layer on the diffusion layer to have a film thickness shown in Table 1. For example, in Example 1, the film thickness of the barrier layer was 9 nm.

[0312] The barrier layer was prepared by digital sputtering using a silicon target at a frequency of 100 kHz and a power density of 10.0 W / cm while maintaining the pressure at 0.2 Pa with argon gas. 2 , pulse sputtering is performed under the condition of inversion pulse width of 3μsec to form a silicon film with a small film thickness, and then nitridation with nitrogen gas is repeated at a high speed to form a silicon nitride film, forming a silicon nitride (SiN) film with a specified film thickness. x Here, the nitrogen flow rate during nitridation with nitrogen gas is 800 sccm, and the input power of the nitridation source is 600W.

[0313] (Formation of anti-reflection film)

[0314] Next, NMWO layers (high refractive index layers) and SiO layers (low refractive index layers) are alternately formed on the barrier layer to form an antireflection film having a film structure shown in Table 1. It should be noted that the NMWO layer refers to a mixed oxide layer of Nb, Mo, and W. For example, the film structure of the antireflection film of Example 1 in Table 1 is to form a 4nm NMWO layer on the barrier layer, then form a 40nm SiO layer, then form a 44nm NMWO layer, then form a 15nm SiO layer, then form a 46nm NMWO layer, and then form an 87nm SiO layer, thereby forming an antireflection film having a film structure consisting of 6 layers. The film forming methods of the SiO layer and the NMWO layer are as follows.

[0315] (Film formation of NMWO layer)

[0316] A target made of niobium, molybdenum, and tungsten mixed and sintered in a mass ratio of 24:30:46 was used by digital sputtering. The pressure was maintained at 0.2 Pa with argon gas and the frequency was 100 kHz and the power density was 10.0 W / cm 2 , pulse sputtering is performed under the condition of an inversion pulse width of 3μsec to form a metal film of a small film thickness, and then oxidation with oxygen is repeated at a high speed to form an oxide film, thereby forming an NMWO layer of a specified film thickness. It should be noted that the composition of the NMWO layer formed by this method is measured by depth direction composition analysis using X-ray photoelectron spectroscopy (XPS) using argon ion sputtering. Excluding oxygen, Nb is 31.5at%, Mo is 38.1at%, W is 30.5at%, and the content of group B elements is 24wt%.

[0317] (SiO layer formation)

[0318] A silicon target was used by digital sputtering, and the pressure was maintained at 0.2 Pa with argon gas at a frequency of 100 kHz and a power density of 10.0 W / cm 2 , pulse sputtering is performed under the condition of inversion pulse width of 3μsec to form a silicon film with a small film thickness, and then it is immediately oxidized with oxygen at a high speed to form a silicon oxide film, forming a silicon oxide film [silicon dioxide (SiO x Here, the oxygen flow rate during the oxidation with oxygen is 500 sccm, and the input power of the oxidation source is 1000W.

[0319] (Formation of antifouling film)

[0320] KY-185 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), a fluorine-containing organosilicon compound, was placed in a metal crucible (evaporation source) and heated and evaporated at 230-350°C. The evaporated particles were evaporated and diffused into a vacuum chamber where a substrate was set and adhered to the surface of the substrate. A 4nm thick antifouling film was formed while monitoring the evaporation rate by controlling the crystal oscillator.

[0321] (Transparent substrates 2 and 3 with anti-reflection films)

[0322] Transparent substrates 2 and 3 with anti-reflection films were obtained in the same manner as transparent substrate 1 with anti-reflection films. However, due to the deviation of film thickness caused by the film forming process, the film thickness of each layer in the anti-reflection film, etc. in transparent substrates 2 and 3 with anti-reflection films is slightly different from that in transparent substrate 1 with anti-reflection films.

[0323] The results of the above evaluations of the transparent substrates 1 to 3 with antireflection films and the unit panels 1 to 3 are shown in Table 1. Here, the unit panels 2 and 3 were evaluated for Δa * b * The results of the difference in reflected color when arranged with the unit panel 1 correspond to the results of the evaluation of the spliced ​​displays of Examples 1 and 2, respectively.

[0324] [Table 1]

[0325]

[0326] The results in Table 1 confirm that in a spliced ​​display (spliced ​​display of Example 1) in which two adjacent unit panels are composed of the unit panels of Example 1 and Example 2 satisfying Condition 1, the difference in reflected color when spliced ​​is hardly noticeable.

[0327] (Examples 3~5)

[0328] The following Examples 3 to 5 are examples according to the above-mentioned second embodiment.

[0329] Unit panels 4 to 7 were prepared respectively, and the spliced ​​displays obtained by combining and arranging them were evaluated. The spliced ​​display combining unit panels 4 and 5 (the spliced ​​display of Example 3) corresponds to the embodiment, and the spliced ​​display combining unit panels 4 and 6 (the spliced ​​display of Example 4), and the spliced ​​display combining unit panels 4 and 7 (the spliced ​​display of Example 5) correspond to the comparative example.

[0330] (evaluate)

[0331] (L of diffuse reflected light * )

[0332] The L value of diffuse reflected light was measured for the transparent substrate with anti-reflection film used in each unit panel according to the following method: * It should be noted that when observing the transparent substrate with the antireflection film, black tape (Kukiri Miel, manufactured by Tomogawa Paper Co., Ltd.) was attached to the main surface on the side without the diffusion layer to remove the reflection on the main surface on the side without the diffusion layer.

[0333] The light source is incident at an incident angle of 45° on the main surface (one main surface) of the transparent substrate with a diffusion layer provided on the display surface side of the unit panel with an anti-reflection film. The reflectance of each diffuse reflection light at an angle of -15° relative to the mirror reflection light is measured for the visible light wavelength, and the L under the D65 light source is calculated. * (Diffuse reflectance) The measurement was performed using CM-M6 manufactured by Konica Minolta Inc. The results of the measurement using the spectrophotometer CM-26d manufactured by Konica Minolta Inc. were the same even though the absolute values ​​of the L* values ​​were different.

[0334] One direction on the main surface of the transparent substrate with an anti-reflection film (corresponding to the 0° direction in the obtained spliced ​​display) is set as the 0° direction, and 36 directions are set as the incident directions at intervals of 10° up to the 360° direction. * Based on the results, the L values ​​of each unit panel in Condition 2 of the obtained spliced ​​display were determined. * The angle in the direction where the value is maximum.

[0335] (Unit Panel 4)

[0336] As an anti-glare film, an anti-glare PET film (manufactured by Reiko Co., Ltd., Sa: 0.259 μm, Sdr: 0.0620, Sdq: 0.361, Spc: 1703 (1 / mm), haze value: 60%) is used, and a barrier layer, an anti-reflection film and an anti-fouling layer are formed on the diffusion layer to obtain a transparent substrate 4 with an anti-reflection film. The method for forming the barrier layer, the anti-reflection film and the anti-fouling layer is the same as that for the transparent substrate 1 with an anti-reflection film. The obtained transparent substrate 4 with an anti-reflection film is bonded to the display surface side of an OLED display (Pixel 6Pro manufactured by Google) which is self-luminous. At this time, the transparent substrate 4 with an anti-reflection film is bonded in such a manner that the MD direction of the anti-glare film is consistent with the upper direction (hereinafter also referred to as the reference direction) in the front view of the display surface of the display, thereby obtaining a unit panel 4.

[0337] (Unit Panel 5, Example 3)

[0338] As an anti-glare film, an anti-glare PET film (manufactured by Reiko Co., Ltd., Sa: 0.259 μm, Sdr: 0.0620, Sdq: 0.361, Spc: 1703 (1 / mm), haze value: 60%) is used, and a barrier layer, an anti-reflection film and an anti-fouling layer are formed on the diffusion layer to obtain a transparent substrate 5 with an anti-reflection film. The method for forming the barrier layer, the anti-reflection film and the anti-fouling layer is the same as that for the transparent substrate 4 with an anti-reflection film. The obtained transparent substrate 5 with an anti-reflection film is bonded to the display surface side of an OLED display (Pixel 6Pro manufactured by Google) which is a self-luminous device. At this time, the transparent substrate 5 with an anti-reflection film is bonded in such a manner that the MD direction of the anti-glare film is consistent with the upper direction (reference direction) in the front view of the display surface of the display, thereby obtaining a unit panel 5. The unit panels 4 and 5 are arranged adjacent to each other to obtain the spliced ​​display of Example 3. It should be noted that the shape of the main surface of the unit panels 4 to 7 is roughly rectangular, and in the spliced ​​displays of Examples 3 to 5, two adjacent unit panels are arranged in a manner that shares one side on their boundary. In addition, in each spliced ​​display, the unit panels are arranged in a manner that the reference direction when the transparent substrate with an anti-reflection film is attached to each unit panel is the same direction in one spliced ​​display. That is, in the spliced ​​display of Example 3, the unit panels are arranged in a manner that the reference direction in the unit panel 4 and the reference direction in the unit panel 5 are the same direction (for example, both are upward directions when viewed from the front of the main surface of the spliced ​​display).

[0339] (Unit Panel 6, Example 4)

[0340] A transparent substrate 5 with an anti-reflection film was used and bonded to the display surface side of a self-luminous OLED display (Pixel 6Pro manufactured by Google). At this time, the MD direction of the anti-glare film was rotated 90° clockwise relative to the upper direction (reference direction) in the front view of the display surface of the display, and the transparent substrate 5 with an anti-reflection film was bonded to obtain a unit panel 6. The unit panels 4 and 6 were arranged adjacent to each other to obtain the spliced ​​display of Example 4.

[0341] (Unit Panel 7, Example 5)

[0342] A transparent substrate 5 with an anti-reflection film is used and bonded to the display surface side of a self-luminous OLED display (Pixel 6Pro manufactured by Google). At this time, the MD direction of the anti-glare film is rotated 180° clockwise relative to the upper direction (reference direction) in the front view of the display surface of the display, and the transparent substrate 5 with an anti-reflection film is bonded to obtain a unit panel 7. The unit panels 4 and 7 are arranged in an adjacent manner to obtain a spliced ​​display of Example 5.

[0343] (Evaluation results)

[0344] The results of the above measurements in each spliced ​​display are shown in Figures 8 to 10 .Right now, Figure 8 The L in the 36 direction of each unit panel (unit panel 4 and 5) in the spliced ​​display of Example 3 is shown. * The value graph, Fig. 9 The L in the 36 direction of each unit panel (unit panels 4 and 6) in the spliced ​​display of Example 4 is shown. * The value graph, Fig.10 The L in the 36 directions of each unit panel (unit panels 4 and 7) in the spliced ​​display of Example 5 is shown. * It should be noted that L * The measured value of the value itself is a value obtained by measuring the transparent substrate with an anti-reflection film used in each unit panel separately. Even in the state of forming a unit panel, the measurement is performed in the same way. The L value based on the incident direction is * The directionality of the value will not change.

[0345] In the spliced ​​display of Example 3, the L of the unit panel 4 * The maximum value is 350°, L * The maximum value is 54.56. L unit panel 5 L * The angle of the direction with the maximum value is 10°, L * The maximum value is 54.32. * The difference in angles in the directions with the largest values ​​is 20°.

[0346] In the spliced ​​display of Example 4, L of unit panel 4 * The maximum value is 350°, L * The maximum value is 54.56. L of unit panel 6 * The angle of the direction with the maximum value is 100°, L * The maximum value is 54.32. * The difference in angles in the directions with the largest value is 120°.

[0347] In the spliced ​​display of Example 5, the L of the unit panel 4 * The maximum value is 350°, L * The maximum value is 54.56. L of unit panel 7 * The angle of the direction with the maximum value is 190°, L * The maximum value is 54.32. * The difference in angles between directions with the largest value is 160°.

[0348] When visually observing the spliced ​​display of Example 3, no difference in hue (reflected color) between the unit panels was detected, regardless of whether it was viewed straight or obliquely. When visually observing the spliced ​​displays of Examples 4 and 5 from various angles, differences in hue (reflected color) between the unit panels were detected, and the color deviation was obvious.

[0349] In the above, various embodiments are described with reference to the accompanying drawings, but it is self-evident that the present invention is not limited to such examples. Obviously, those skilled in the art can think of various variations or modifications within the scope of the patent application, which of course also belong to the technical scope of the present invention. In addition, the various constituent elements in the above embodiments may also be combined arbitrarily without departing from the scope of the invention.

[0350] It should be noted that the present application is based on the Japanese patent application filed on April 8, 2022 (Japanese Patent Application No. 2022-064751), the Japanese patent application filed on April 8, 2022 (Japanese Patent Application No. 2022-064752), the Japanese patent application filed on July 13, 2022 (Japanese Patent Application No. 2022-112709), and the Japanese patent application filed on November 29, 2022 (Japanese Patent Application No. 2022-190437), the contents of which are incorporated into the present application by reference.

[0351] Explanation of symbols

[0352] 100, 200 splicing display

[0353] 5, 5a, 5b, 205, 205a, 205b unit panels

[0354] 7, 7a, 7b, 207, 207a, 207b main body

[0355] 1. 1a, 1b Transparent substrate with anti-reflection film

[0356] 201, 201a, 201b anti-glare film

[0357] 10 Transparent substrate

[0358] 210 resin matrix

[0359] 11 A main surface

[0360] 12 Another main face

[0361] 20 black tape

[0362] 30 Anti-reflective film

[0363] 31, 231 diffusion layer

[0364] 321st dielectric layer

[0365] 34 2nd dielectric layer

[0366] 50 light sources

[0367] 60Incident light

[0368] 61 Specular reflection light

[0369] 71, 72, 73, 74, 75, 76 Diffuse reflected light

[0370] 80 incident light

[0371] 81 Diffuse light

[0372] D1 0° direction

[0373] S The edge shared by two adjacent unit panels

[0374] P Projection Trajectory

Claims

1. A spliced ​​display, comprising a plurality of unit panels having a transparent substrate with an anti-reflection film on the display surface side, The transparent substrate with anti-reflection film has a transparent substrate, a diffusion layer and an anti-reflection film in sequence toward the display surface. The two adjacent unit panels satisfy the following condition 1: Condition 1 When a light source is incident on the main surface of one of the two unit panels at a 45° incident angle, diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light is reflected under a D65 light source. * and b * Let a be the value of each angle x * and b x * , the same measurement of a on another unit panel * and b * Let a be the value of each angle y * and b y * When Δa of each angle * b * is below 3.0, Δa * b * =((a x * -a y * ) 2 +(b x * -b y * ) 2 ) 1 / 2 。 2. The spliced ​​display according to claim 1, wherein: The transparent substrate with an antireflection film has a haze value of 30% or more.

3. A unit panel set for a spliced ​​display composed of a plurality of unit panels each having a transparent substrate with an anti-reflection film on the display surface side, The transparent substrate with anti-reflection film has a transparent substrate, a diffusion layer and an anti-reflection film in sequence toward the display surface. Two unit panels selected from the unit panel group satisfy the following condition 1, Condition 1 When a light source is incident on the main surface of one of the two unit panels at a 45° incident angle, diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light is reflected under a D65 light source. * and b * Let a be the value of each angle x * and b x * , the same measurement of a on another unit panel * and b * Let a be the value of each angle y * and b y * When Δa of each angle * b * is below 3.0, Δa * b * =((a x * -a y * ) 2 +(b x * -b y * ) 2 ) 1 / 2 。 4. The unit panel set according to claim 3, wherein: The transparent substrate with an antireflection film has a haze value of 30% or more.

5. A method for manufacturing a spliced ​​display, which is a method for manufacturing a spliced ​​display formed by arranging a plurality of unit panels having a transparent substrate with an anti-reflection film on the display surface side, comprising: For a plurality of the unit panels, when a light source is incident on the main surface on the display surface side at an incident angle of 45°, the a value of the diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light under a D65 light source is determined. * and b * , A combination of unit panels satisfying the following condition 1 is selected, and the unit panels satisfying the combination are arranged so as to be adjacent to each other. Condition 1 When a light source is incident on the main surface of one of the two unit panels at a 45° incident angle, diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light is reflected under a D65 light source. * and b * Let a be the value of each angle x * and b x * , the same measurement of a on another unit panel * and b * Let a be the value of each angle y * and b y * When Δa of each angle * b * is below 3.0, Δa * b * =((a x * -a y * ) 2 +(b x * -b y * ) 2 ) 1 / 2 。 6. A maintenance method for a spliced ​​display, which is a maintenance method for a spliced ​​display composed of a plurality of unit panels having a transparent substrate with an anti-reflection film on the display surface side, comprising: Select the unit panel to be replaced from the unit panels that constitute the tiled display. For at least one adjacent unit panel adjacent to the unit panel to be replaced, when a light source is incident on the main surface on the display surface side at an incident angle of 45°, the a value of the diffuse reflected light under a D65 light source at angles of -15°, 15°, and 25° relative to the specular reflected light is confirmed. * and b * , The unit panel to be replaced is replaced in such a manner that the replaced unit panel satisfies the following condition 1 with respect to the adjacent unit panel, Condition 1 When a light source is incident on the main surface of one of the two unit panels at a 45° incident angle, diffuse reflected light at angles of -15°, 15°, and 25° relative to the specular reflected light is reflected under a D65 light source. * and b * Set a at each angle x * and b x * , the same measurement of a on another unit panel * and b * Set a at each angle y * and b y * When Δa of each angle * b * is below 3.0, Δa * b * =((a x * -a y * ) 2 +(b x * -b y * ) 2 ) 1 / 2 。 7. The spliced ​​display according to claim 1 or 2, wherein: The transparent substrate with an anti-reflection film comprises an anti-glare film as the diffusion layer and the transparent substrate, The two adjacent unit panels satisfy the following condition 2: Condition 2 The L of one of the two adjacent unit panels is obtained using the following method * The angle in the direction with the maximum value is the same as the L measured for the other unit panel. * The angle difference in the direction with the largest value is less than 35°. method On a surface parallel to the main surface of the spliced ​​display, one of the directions parallel to the sides shared by the two adjacent unit panels is set as the 0° direction, and the light source is incident on the main surface of the display surface side of the unit panel as the measurement object at a 45° incident angle, and the incident direction is changed from the 0° direction to the 360° direction at 10° intervals, and the L value of the diffuse reflected light at an angle of -15° relative to the specular reflected light of the incident light under the D65 light source is measured in each incident direction. * value, L * The value is the maximum incident angle L of the unit panel to be measured. * The angle in the direction where the value is maximum.

8. A spliced ​​display, comprising a plurality of unit panels having an anti-glare film on the display surface side, The two adjacent unit panels satisfy the following condition 2: Condition 2 The L of one of the two adjacent unit panels is obtained using the following method * The angle in the direction with the maximum value is the same as the L measured for the other unit panel. * The angle difference in the direction with the largest value is less than 35°. method On a surface parallel to the main surface of the spliced ​​display, one of the directions parallel to the sides shared by the two adjacent unit panels is set as the 0° direction, and the light source is incident on the main surface of the display surface side of the unit panel as the measurement object at a 45° incident angle, and the incident direction is changed from the 0° direction to the 360° direction at 10° intervals, and the L value of the diffuse reflected light at an angle of -15° relative to the specular reflected light of the incident light under the D65 light source is measured in each incident direction. * value, L * The value is the maximum incident angle L of the unit panel to be measured. * The angle in the direction where the value is maximum.

9. A method for manufacturing a spliced ​​display, which is a method for manufacturing a spliced ​​display formed by arranging a plurality of unit panels having an anti-glare film on the display surface side, comprising: The unit panels are configured so that adjacent unit panels satisfy the following condition 2: Condition 2 The L of one of the two adjacent unit panels is obtained using the following method * The angle in the direction with the maximum value is the same as the L measured for the other unit panel. * The angle difference in the direction with the largest value is less than 35°. method On a surface parallel to the main surface of the spliced ​​display, one of the directions parallel to the sides shared by the two adjacent unit panels is set as the 0° direction, and the light source is incident on the main surface of the display surface side of the unit panel as the measurement object at a 45° incident angle, and the incident direction is changed from the 0° direction to the 360° direction at 10° intervals, and the L value of the diffuse reflected light at an angle of -15° relative to the specular reflected light of the incident light under the D65 light source is measured in each incident direction. * value, L * The value is the maximum incident angle L of the unit panel to be measured. * The angle in the direction where the value is maximum.

10. A maintenance method for a spliced ​​display, which is a maintenance method for a spliced ​​display formed by arranging a plurality of unit panels having an anti-glare film on the display surface side, comprising: Select the unit panel to be replaced from among the unit panels that constitute the tiled display. The unit panel to be replaced is replaced in such a manner that the replaced unit panel satisfies the following condition 2 with respect to at least one adjacent unit panel adjacent to the unit panel to be replaced, Condition 2 The L of one of the two adjacent unit panels is obtained using the following method * The angle in the direction with the maximum value is the same as the L measured for the other unit panel. * The angle difference in the direction with the largest value is less than 35°. method On a surface parallel to the main surface of the spliced ​​display, one of the directions parallel to the sides shared by the two adjacent unit panels is set as the 0° direction, and the light source is incident on the main surface of the display surface side of the unit panel as the measurement object at a 45° incident angle, and the incident direction is changed from the 0° direction to the 360° direction at 10° intervals, and the L value of the diffuse reflected light at an angle of -15° relative to the specular reflected light of the incident light under the D65 light source is measured in each incident direction. * value, L * The value is the maximum incident angle L of the unit panel to be measured. * The angle in the direction where the value is maximum.

Citation Information

Patent Citations

  • Display module and display device having the same

    CN112992962A

  • Film-based frontlight with angularly varying diffusion film

    CN113272693A

  • Tiled electronic display structure

    CN1291353A

  • Direct view type display device

    JP2001265240A

  • Display panel and display

    JP2019020486A