SCR catalyst and preparation method thereof

An SCR catalyst was prepared by using untreated red mud with cerium nitrate hexahydrate and tetrabutyl titanate. This solved the temperature window and poisoning resistance problems of existing catalysts, realizing the resource utilization of red mud and efficient denitrification, which is suitable for industrial applications.

CN118976480AInactive Publication Date: 2024-11-19SICHUAN NORMAL UNIV +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411079298.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing SCR catalysts suffer from problems such as high temperature window, poor resistance to poisoning, V2O5 biotoxicity, and small specific surface area. Traditional catalysts are difficult to promote and use in industry, and acid washing during the preparation of red mud causes secondary pollution.

Method used

A catalyst was prepared by ball milling and calcination using untreated red mud, cerium nitrate hexahydrate, and tetrabutyl titanate as raw materials to increase the specific surface area and expose active sites. The addition of cerium and titanium elements improved the resistance to poisoning.

Benefits of technology

The prepared SCR catalyst exhibits good denitrification effect at medium and low temperatures, promotes the resource utilization of red mud, has no secondary pollution, and has industrial application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an SCR catalyst and a preparation method thereof, and relates to the technical field of catalyst preparation, the SCR catalyst comprises the following raw materials: red mud, cerium nitrate hexahydrate and tetrabutyl titanate, the mass ratio of the red mud to the cerium nitrate hexahydrate to the tetrabutyl titanate in the SCR catalyst is 1: 0.06-0.13: 0.07-0.16, and the red mud adopts raw red mud which is not subjected to acid treatment. The SCR catalyst is prepared from the primary red mud, secondary environmental pollution is not generated, resource utilization of the red mud is promoted, and the catalyst can be used for denitration at the temperature of 200 DEG C or above, has good economical efficiency and has practical application value in industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst preparation, and in particular to an SCR catalyst and a preparation method thereof. Background Art

[0002] Nitrogen oxides (NO x ) is one of the main air pollutants, causing a series of environmental problems such as acid rain, photochemical smog and greenhouse effect, and also causing harm to human health. Fixed pollution sources such as coal-fired power plants and mobile pollution sources such as automobile exhaust continue to emit large amounts of NO x Environmental regulations on NO in flue gas x The residual volume is more strictly controlled to eliminate NO x It is still a hot topic in current research. x Selective catalytic reduction to N2 and H2O is an environmentally friendly, stable and reliable technology.

[0003] At present, the most widely used industrial catalyst in the SCR denitrification system is the V-Ti-W series catalyst, but it still has disadvantages such as high temperature window, poor anti-poisoning ability and biological toxicity of V2O5. At the same time, traditional catalysts have problems such as small specific surface area and difficult porosity control, which limits industrial application. Therefore, relevant researchers have focused on the development of new environmentally friendly NH3-SCR reaction catalysts. In recent years, the excellent performance of red mud (RM) catalysts in the medium and high temperature range (>300℃) and good SO2 resistance in NH3-SCR reactions have attracted widespread attention. However, the pH value of raw red mud is in the range of 12~14, which is a kind of alkaline solid waste. In the process of preparing catalysts from raw red mud, it is generally necessary to acid wash it, because ordinary water washing can only remove free alkali, while acid washing can convert bonded alkali into free alkali and then remove it. At the same time, acid washing removes alkaline heavy metals such as K and Na to avoid forming corresponding metal salts with SO2 to block pores and shield active sites, reduce the probability of catalyst poisoning, and thus improve the denitrification efficiency of the catalyst. However, the dealkalization of red mud involves the use of large amounts of acidic substances, poor operability, and large amounts of waste liquid, which can easily cause secondary pollution, making it difficult to promote its use. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide an SCR catalyst and a preparation method thereof.

[0005] The objective of the present invention is achieved through the following technical solutions: A SCR catalyst is composed of the following raw materials: red mud, cerium nitrate hexahydrate and tetrabutyl titanate. The mass ratio of the red mud, cerium nitrate hexahydrate and tetrabutyl titanate in the SCR catalyst is 1:0.06-0.13:0.07-0.16, and the red mud is primary red mud that has not been treated with acid.

[0006] The preparation method of the above-mentioned SCR catalyst comprises the following steps: S1, ball-milling red mud, cerium nitrate hexahydrate and tetrabutyl titanate to obtain a catalyst precursor; S2. The catalyst precursor is ground and passed through a 80-120 mesh sieve, and calcined at 380-420° C. for 3 hours to obtain an SCR catalyst.

[0007] The ball milling speed during ball milling in S1 was 420 r / min, and the ball milling time was one hour.

[0008] Zirconium balls were added during ball milling in S1.

[0009] The calcination temperature in S2 is increased at a rate of 5°C / min.

[0010] There are two main reactions involved in its use: Common reaction: 4NO + 4NH3 + O2 = 4N2 + 6H2O Fast reaction: 6NO2 + 8NH3 = 7N2 + 12H2O The invention adopts mechanical ball milling to increase the specific surface area of ​​the catalyst. Ball milling also breaks up the red mud, destroys the crystal structure of the structural alkaline substances, and exposes the alkaline substances to react with NO to generate nitrate or nitrite. The cerium and titanium elements added during ball milling make the catalyst surface have more Lewis acid sites, making it easier to adsorb NH3 to generate -NH2 or NH4 + , substances adsorbed on the catalyst surface are more likely to react and generate nitrogen and water. The introduction of cerium and titanium elements also promotes the increase of oxygen adsorbed on the catalyst surface, NO is oxidized to NO2, and a rapid SCR reaction is more likely to occur. At the same time, cerium and titanium elements can act as sacrificial agents to improve the anti-poisoning ability of the catalyst.

[0011] The beneficial effects of the present invention are: (1) The SCR catalyst in the present invention is prepared from primary red mud, does not cause secondary environmental pollution, promotes the resource utilization of red mud, and the catalyst can denitrify at 200°C or above, has good economic efficiency, and has practical application value in industry.

[0012] (2) The SCR catalyst synthesis method of the present invention is simple and easy, and red mud is widely available. A trace amount of cerium nitrate hexahydrate and tetrabutyl titanate are added to obtain a precursor by a simple ball milling method. DETAILED DESCRIPTION

[0013] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0014] The red mud used in the embodiments of the present invention is all original red mud that has not been treated with acid.

[0015] Example 1 A method for preparing an SCR catalyst, characterized in that it comprises the following steps: S1. Preparation of catalyst precursor by ball milling 3.5 g of red mud, 0.42 g of cerium nitrate hexahydrate and 0.5 g of tetrabutyl titanate were added to a ball mill filled with zirconium beads (11 beads with a diameter of 10 mm, 12 beads with a diameter of 5 mm and 15 beads with a diameter of 3 mm). The mixture was ball milled at a speed of 420 r / min for one hour to obtain a catalyst precursor; S2. Preparation of SCR catalyst The catalyst precursor was ground through a 100-mesh sieve and then placed in an ark. The temperature was raised to 400° C. at 5° C. / min in a muffle furnace, and the SCR catalyst was calcined at 400° C. for 3 hours.

[0016] Example 2 A method for preparing an SCR catalyst, characterized in that it comprises the following steps: S1. Preparation of catalyst precursor by ball milling 3.5 g of red mud, 0.42 g of cerium nitrate hexahydrate and 0.25 g of tetrabutyl titanate were added to a ball mill filled with zirconium beads (11 beads with a diameter of 10 mm, 12 beads with a diameter of 5 mm and 15 beads with a diameter of 3 mm). The mixture was ball milled at a speed of 420 r / min for one hour to obtain a catalyst precursor; S2. Preparation of SCR catalyst The catalyst precursor was ground through a 80-mesh sieve and then placed in an ark. The temperature was raised to 410° C. at 5° C. / min in a muffle furnace, and the SCR catalyst was calcined at 410° C. for 3 hours.

[0017] Example 3 A method for preparing an SCR catalyst, characterized in that it comprises the following steps: S1. Preparation of catalyst precursor by ball milling 3.5 g of red mud, 0.21 g of cerium nitrate hexahydrate and 0.5 g of tetrabutyl titanate were added to a ball mill filled with zirconium beads (11 beads with a diameter of 10 mm, 12 beads with a diameter of 5 mm and 15 beads with a diameter of 3 mm). The mixture was ball milled at a speed of 420 r / min for one hour to obtain a catalyst precursor; S2. Preparation of SCR catalyst The catalyst precursor was ground through a 90-mesh sieve and then placed in an ark. The temperature was raised to 380° C. at 5° C. / min in a muffle furnace, and the SCR catalyst was calcined at 380° C. for 3 hours.

[0018] Example 4 A method for preparing an SCR catalyst, characterized in that it comprises the following steps: S1. Preparation of catalyst precursor by ball milling 3.5 g of red mud, 0.21 g of cerium nitrate hexahydrate and 0.25 g of tetrabutyl titanate were added to a ball mill filled with zirconium beads (11 beads with a diameter of 10 mm, 12 beads with a diameter of 5 mm and 15 beads with a diameter of 3 mm). The mixture was ball milled at a speed of 420 r / min for one hour to obtain a catalyst precursor; S2. Preparation of SCR catalyst The catalyst precursor was ground through a 110-mesh sieve and then placed in an ark. The temperature was raised to 390° C. at 5° C. / min in a muffle furnace, and the SCR catalyst was calcined at 390° C. for 3 hours.

[0019] Example 5 A method for preparing an SCR catalyst, characterized in that it comprises the following steps: S1. Preparation of catalyst precursor by ball milling 3.15 g of red mud, 0.42 g of cerium nitrate hexahydrate and 0.5 g of tetrabutyl titanate were added to a ball mill filled with zirconium beads (11 beads with a diameter of 10 mm, 12 beads with a diameter of 5 mm and 15 beads with a diameter of 3 mm). The mixture was ball milled at a speed of 420 r / min for one hour to obtain a catalyst precursor; S2. Preparation of SCR catalyst The catalyst precursor was ground through a 120-mesh sieve and then placed in an ark. The temperature was raised to 420° C. at 5° C. / min in a muffle furnace, and the SCR catalyst was calcined at 420° C. for 3 hours.

[0020] Nitric oxide removal rate test experiment 3.0 g of the catalyst prepared in Examples 1, 2, 3, 4, and 5 was weighed for experiment. The experimental conditions were set as [NO] = 600 ppm, [NH3] = 600 ppm, [O2] = 6 vol%, GHSV = 30000 h −1. The total flow rate is 500mL / min, the inner diameter of the reactor is 6mm, and the material filling height is 3.5cm. Experimental exploration of different materials was carried out by setting a temperature gradient. When the temperature was 60℃, 80℃, 120℃, 160℃, 200℃, and 240℃, each temperature interval was maintained for 30min. The average value of the temperature interval was taken for each embodiment to record the experimental data. The results are shown in Table 1. The nitrogen monoxide removal rate of the SCR catalyst was calculated based on the data recorded by the flue gas analyzer. At 240℃, the nitrogen monoxide removal rate reached 80% or more.

[0021] Table 1 Nitric oxide removal rate data results Experimental conclusion: The SCR catalyst provided by the present invention promotes the resource utilization of red mud without dealkalization and has a good catalytic effect at medium and low temperatures.

[0022] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. An SCR catalyst, It is characterized in that The SCR catalyst is composed of the following raw materials: red mud, cerium nitrate hexahydrate and tetrabutyl titanate. The mass ratio of red mud, cerium nitrate hexahydrate and tetrabutyl titanate in the SCR catalyst is 1:0.06-0.13:0.07-0.

16. The red mud is original red mud that has not been treated with acid.

2. A method for preparing the SCR catalyst according to claim 1, Features: The following steps are involved: S1, ball-milling red mud, cerium nitrate hexahydrate and tetrabutyl titanate to obtain a catalyst precursor; S2. The catalyst precursor is ground and sieved, and calcined at 380-420° C. for 3 hours to obtain an SCR catalyst.

3. The preparation method according to claim 2, Features: The ball milling speed during the ball milling in S1 is 420 r / min, and the ball milling time is one hour.

4. The preparation method according to claim 2, Features: Zirconium balls were added during the ball milling described in S1.

5. The preparation method according to claim 2, Features: After grinding in S2, pass through a 80-120 mesh sieve.

6. The preparation method according to claim 2, Features: The calcination temperature in S2 is increased at a rate of 5°C / min.

Citation Information

Patent Citations

  • Iron, cerium and red mud composite oxide denitration catalyst material and preparation method thereof

    CN106238064A

  • Red mud-based denitration catalyst as well as preparation method and applications thereof

    CN110479247A

  • Preparation method of novel modified red mud-based denitration catalyst

    CN116116418A

  • Supported molten-metal catalysts

    US6218326B1