Nickel-based cerium dioxide hollow sphere catalyst as well as preparation method and application thereof
The preparation of nickel-based ceria hollow sphere catalysts by solvent thermal method solves the problems of high catalytic temperature and poor catalytic activity in the prior art, and realizes low-temperature catalytic and efficient carbon dioxide methanation reactions, which significantly improves the performance of the catalyst.
Patent Information
- Application Number
- CN202410803088.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-19
AI Technical Summary
The existing nickel-based ceria catalysts have high catalytic temperature and poor catalytic activity in carbon dioxide methanation reaction, and lack high specific surface area and low temperature catalytic properties.
The nickel-based ceria hollow sphere catalyst was prepared by solvent-heating method, and mesoporous ceria hollow spheres were prepared by surfactant and supported by nickel oxide or metal nickel to form a uniform hollow sphere morphology and large specific surface area, thereby improving the adsorption of the catalyst. Capacity and catalytic performance.
The temperature required for catalytic reaction is reduced, the catalytic activity and conversion and selectivity of carbon dioxide methanation are improved, and the performance of the catalyst is significantly improved.
Smart Images

Figure CN118976502A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and specifically relates to a nickel-based cerium dioxide hollow sphere catalyst and a preparation method and application thereof. Background Art
[0002] Since the Industrial Revolution, people's demand for fossil fuels such as coal, oil, and natural gas has increased dramatically. The continuous consumption of fossil fuels has caused a global energy crisis and greenhouse gas carbon dioxide emissions, which has caused global warming, leading to drastic climate changes and various natural disasters, seriously threatening the survival of humans and other organisms. Therefore, exploring new technologies for the conversion, reuse, and clean energy production of carbon dioxide is of great research significance for effectively reducing carbon dioxide emissions. So far, carbon dioxide chemical conversion technology is considered to be one of the most important and feasible methods to reduce carbon emissions. In addition, methane is an important component of natural gas, its combustion products are clean and safe, and can be transported through existing pipelines. Therefore, from the perspectives of energy and environment, carbon dioxide hydrogenation to methane has a very broad application prospect.
[0003] At present, the core technology of the reported carbon dioxide hydrogenation to methane lies in the selection of catalysts. Carbon dioxide methanation catalysts can be divided into two categories: precious metal-based catalysts and non-precious metal-based catalysts. Among them, precious metal-based catalysts are often expensive and have too high a recycling cost. Non-precious metal nickel-based catalysts have attracted widespread attention due to their high catalytic activity in the carbon dioxide methanation reaction, as well as their low price and abundant resources. Ceria has been widely used in optimizing nickel-based carbon dioxide methanation catalysts due to its good chemical stability, carbon dioxide adsorption performance and excellent oxygen storage and release capacity. However, in the prior art, nickel-based ceria catalysts usually have a small specific surface area (40-70 m 2 / g), high catalytic reaction temperature (300-600 ℃) and poor catalytic activity. Therefore, a nickel-based-cerium dioxide catalyst with high specific surface area, low-temperature catalysis and high catalytic activity is developed, which has good application prospects in the carbon dioxide methanation reaction. Summary of the invention
[0004] The purpose of the present invention is to solve the defects of the prior art such as the high catalytic temperature required for the carbon dioxide methanation reaction and the poor performance of the existing nickel-based catalyst, and provide a nickel-based cerium dioxide hollow sphere catalyst and a preparation method and application thereof. The catalyst contains mesoporous cerium dioxide hollow spheres and active components such as metal nickel and / or nickel oxide loaded on the mesoporous cerium dioxide hollow spheres. The catalyst has a uniform hollow sphere morphology and a large specific surface area, which is conducive to the formation of oxygen vacancies and the uniform dispersion of the nickel-based active components, thereby improving the adsorption capacity of the catalyst for carbon dioxide and the catalytic performance of catalyzing carbon dioxide methanation. The method uses a solvent thermal method and a surfactant to prepare the cerium dioxide hollow spheres, thereby avoiding the use of a template and being simple to operate. At the same time, the hollow structure of the cerium dioxide hollow spheres can effectively protect the catalyst and avoid thermal sintering of the catalyst in a high temperature environment, thereby facilitating the preparation of a nickel-based cerium dioxide hollow sphere catalyst with a large specific surface area, improving the catalytic activity of the catalyst and reducing the temperature required for the carbon dioxide methanation reaction.
[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a nickel-based ceria hollow sphere catalyst, wherein the catalyst comprises ceria hollow spheres and an active component supported on the hollow spheres; Wherein, the hollow cerium dioxide sphere is a mesoporous material; The active component is nickel oxide and / or metallic nickel; The specific surface area of the catalyst is 80-120 m 2 / g.
[0006] Preferably, the catalyst has a pore size of 2-10 nm and a pore volume of 0.05-0.5 cm 3 / g.
[0007] Preferably, in the catalyst, the molar ratio of nickel element to cerium dioxide is 4-8:1.
[0008] The second aspect of the present invention provides a method for preparing a nickel-based cerium dioxide hollow sphere catalyst, characterized in that the method comprises the following steps: Step 1, mixing a surfactant, a cerium salt, a solvent and an acid source and standing them to react, then separating the solid and the liquid and calcining the obtained solid product to obtain cerium dioxide hollow spheres; Step 2, loading nickel salt onto the cerium dioxide hollow spheres obtained in step (1), then performing solid-liquid separation and calcining the obtained solid product; Step 3: Optionally, the product obtained in step 2 is subjected to reduction activation.
[0009] Preferably, in step 1, the surfactant is polyvinyl pyrrolidone.
[0010] Preferably, in step 1, the cerium salt is cerium nitrate.
[0011] Preferably, in step 1, the solvent is ethylene glycol.
[0012] Preferably, in step 1, the acid source is hydrochloric acid.
[0013] Preferably, in step 1, the concentration of the acid source is 0.5-1.5 mol / L.
[0014] Preferably, in step 1, the molar ratio of the acid source, the surfactant and the cerium salt solvent is 1-5:4-8:4-8:1.
[0015] Preferably, in step 1, the reaction conditions include: temperature of 100-250° C., and time of 1-6 h.
[0016] Preferably, in step 2, the loading method is an equal volume impregnation method or a deposition-precipitation method.
[0017] Preferably, in step 2, the nickel salt is nickel nitrate.
[0018] Preferably, in the preparation method described above, when step 2 is an equal volume impregnation method, the steps include: S2, mixing the nickel salt solution and the cerium dioxide hollow spheres obtained in step 1, then performing solid-liquid separation and calcining the obtained solid product.
[0019] Preferably, in S2, the molar ratio of the cerium dioxide hollow spheres to the nickel salt is 1-4:1 Preferably, in the preparation method described above, when step 2 is a deposition-precipitation method, the steps include: (2) Mixing the nickel salt solution, the alkali source and the cerium dioxide hollow spheres obtained in step 1 for reaction, then performing solid-liquid separation and calcining the obtained solid product.
[0020] Preferably, in step (2), the alkali source is sodium hydroxide solution.
[0021] Preferably, in step (2), the concentration of the alkali source solution is 6-9 mol / L.
[0022] Preferably, in step (2), the concentration of the nickel salt solution is 0.3-1 mol / L.
[0023] Preferably, in step (2), the molar ratio of the nickel salt, the alkali source and the cerium dioxide hollow spheres is 1-4:40-60:1.
[0024] Preferably, in step (2), the reaction conditions include: temperature of 50-120°C and time of 10-30 h.
[0025] Preferably, in step 1 and step 2, the calcination conditions include: temperature of 400-600° C. and time of 2-6 hours.
[0026] Preferably, step 2 further comprises performing reduction activation on the obtained calcined product.
[0027] Preferably, in step 2, the reduction activation is carried out under a reducing atmosphere, and the conditions of the reduction activation include: a temperature of 400-550° C., a time of 1-5 h, and a reducing gas space velocity of 15-25 mL / min.
[0028] Preferably, in step 2, the reducing atmosphere is pure hydrogen.
[0029] The present invention also provides a nickel-based cerium dioxide hollow sphere catalyst prepared by the method described above.
[0030] The present invention also provides an application of the nickel-based cerium dioxide hollow sphere catalyst described above in low-temperature catalytic carbon dioxide methanation.
[0031] Compared with the prior art, the present invention has at least the following advantages: (1) In the present invention, the catalyst comprises hollow cerium dioxide spheres and active components nickel oxide and / or metallic nickel supported on the hollow cerium dioxide spheres. The catalyst has a uniform hollow sphere morphology, a low density, good permeability and a large specific surface area (80-120 m 2 / g), and at the same time, in the catalyst, the hollow structure of the mesoporous cerium dioxide nano hollow spheres is conducive to the diffusion of gaseous reactants, the large specific surface area is conducive to the high dispersion of nickel-based active components and the formation of oxygen vacancies, and the uniform pore structure is conducive to the adsorption and desorption of reactants, thereby helping to improve the catalyst's adsorption capacity for carbon dioxide and the catalytic performance of catalyzing carbon dioxide methanation, reduce the temperature required for the catalytic reaction, and improve the catalytic activity.
[0032] (2) In the present invention, the preparation method of the catalyst avoids the use of a PPMA template and is simple to operate. At the same time, the hollow structure of the ceria hollow sphere can effectively protect the catalyst and prevent the catalyst from being thermally sintered under high temperature conditions, thereby facilitating the preparation of a nickel-based ceria hollow sphere catalyst with a large specific surface area, thereby improving the catalytic activity of the catalyst and reducing the temperature required for the carbon dioxide methanation reaction. In a preferred embodiment, nickel is loaded onto the ceria hollow sphere by an isovolumetric impregnation method, which can further increase the specific surface area of the catalyst, significantly improving the nickel-based ceria catalyst in the prior art.
[0033] (3) In the present invention, the catalyst can be used in the low-temperature catalytic carbon dioxide methanation reaction. Compared with the prior art, the catalyst can optimize the reaction kinetics, effectively reduce the temperature required for the catalytic reaction to 250-450 °C, and at the same time improve the conversion rate and selectivity of the carbon dioxide methanation reaction catalyzed by the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 1 is the XRD spectra of the products prepared in Example 1 and Example 2, wherein Figure (a) is the catalyst before reduction activation, and Figure (b) is the catalyst after reduction activation; Figure 2 are SEM images and TEM images of the unactivated catalysts prepared in Example 1 and Example 2, wherein (A1) and (A2) are SEM images and TEM images of the product prepared in Example 1, and (B1) and (B2) are SEM images and TEM images of the product prepared in Example 2; Figure 3 3 is a graph showing the relationship between the carbon dioxide conversion rate and methanation selectivity of the activated catalyst prepared in Example 1 and Example 2 and the reaction temperature. DETAILED DESCRIPTION
[0035] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0036] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0037] The first aspect of the present invention provides a nickel-based ceria hollow sphere catalyst, the catalyst comprising ceria hollow spheres and an active component supported on the hollow spheres; Wherein, the hollow cerium dioxide sphere is a mesoporous material; The active component is nickel oxide and / or metallic nickel; The specific surface area of the catalyst is 80-120 m 2 / g.
[0038] In a preferred embodiment, the specific surface area of the catalyst is 90-120 m 2 / g.
[0039] In the present invention, the catalyst has a uniform hollow spherical morphology, a low density, good permeability and a large specific surface area (80-120 m 2 / g), and at the same time, in the catalyst, the hollow structure of the mesoporous cerium dioxide hollow nanospheres is conducive to the diffusion of gaseous reactants, and the large specific surface area is conducive to the high dispersion of nickel-based active components on the inner and outer surfaces of the mesoporous cerium dioxide hollow nanospheres and the formation of oxygen vacancies in the catalyst, which is conducive to improving the adsorption capacity of the catalyst for carbon dioxide, as well as the catalytic performance of catalyzing carbon dioxide methanation, reducing the temperature required for the catalytic reaction, and improving the catalytic activity.
[0040] In a specific embodiment, the catalyst has a pore size of 2-10 nm and a pore volume of 0.05-0.5 cm 3 / g.
[0041] In a preferred embodiment, the catalyst has a pore size of 3-4 nm and a pore volume of 0.1-0.3 cm 3 Through this preferred embodiment, the catalyst has a uniform and complex pore structure, which is beneficial to the adsorption and desorption of reactants, increases the specific surface area of the catalyst, and improves the catalytic performance of the catalyst.
[0042] In a specific embodiment, in the catalyst, the molar ratio of nickel element to cerium dioxide is 4-8:1.
[0043] In a preferred embodiment, the molar ratio of nickel element to cerium dioxide in the catalyst is 5-6: 1. According to this preferred embodiment, the nickel-based active component in the catalyst can be evenly dispersed on the inner and outer surfaces of the mesoporous cerium dioxide hollow nanospheres, which is beneficial to improve the reaction activity of the catalyst.
[0044] The second aspect of the present invention provides a method for preparing a nickel-based cerium dioxide hollow sphere catalyst, characterized in that the method comprises the following steps: Step 1, mixing a surfactant, a cerium salt, a solvent and an acid source and standing them to react, then separating the solid and the liquid and calcining the obtained solid product to obtain cerium dioxide hollow spheres; Step 2, loading nickel salt onto the cerium dioxide hollow spheres obtained in step (1), then performing solid-liquid separation and calcining the obtained solid product; Step 3: Optionally, the product obtained in step 2 is subjected to reduction activation.
[0045] In the present invention, the method avoids the use of a PPMA template and is simple to operate. At the same time, the hollow structure of the ceria hollow sphere can effectively protect the catalyst and prevent the catalyst from being thermally sintered in a high-temperature environment, thereby facilitating the acquisition of a nickel-based ceria hollow sphere catalyst with a large specific surface area, thereby improving the catalytic activity of the catalyst and reducing the temperature required for the carbon dioxide methanation reaction.
[0046] In a specific embodiment, step 1 further comprises: washing and drying the obtained solid product after solid-liquid separation. In a preferred embodiment, in step 1, the washing is specifically: washing three times by cross centrifugation using ultrapure water and anhydrous ethanol.
[0047] In a preferred embodiment, in step 1, the drying conditions include: a temperature of 50-70°C and a time of 8-16 h. In a further preferred embodiment, the drying conditions include: a temperature of 60°C and a time of 11-13 h.
[0048] In a specific embodiment, step 1 includes the following steps: adding a surfactant and a cerium salt into a solvent and dissolving them, adding an acid source to the resulting solution after complete dissolution, stirring and mixing, and then standing to react, after the reaction is completed, separating the solid and liquid and washing and drying the resulting product, and calcining the dried product to obtain mesoporous cerium dioxide hollow nanospheres.
[0049] In a specific embodiment, in step 1, the surfactant can be selected from conventional sources in the art, as long as the purpose of the present invention can be achieved. In a preferred embodiment, the surfactant can be polyvinyl pyrrolidone.
[0050] In a specific embodiment, in step 1, the cerium salt can be any conventionally selected salt in the art, as long as the purpose of the present invention can be achieved. In a preferred embodiment, the cerium salt can be cerium nitrate or cerium nitrate hexahydrate.
[0051] In a specific embodiment, in step 1, the solvent can be any conventional solvent in the art, as long as the purpose of the present invention can be achieved. In a preferred embodiment, the solvent can be ethylene glycol.
[0052] In a specific embodiment, in step 1, the acid source can be any conventional acid in the art, as long as the purpose of the present invention can be achieved. In a preferred embodiment, the acid source can be hydrochloric acid.
[0053] In a preferred embodiment, the concentration of the acid source may be 0.5-1.5 mol / L.
[0054] In a specific embodiment, in step 1, the molar ratio of the acid source, the surfactant, and the cerium salt solvent is 1-5:4-8:4-8:1. In a preferred embodiment, in step 1, the molar ratio of the acid source, the surfactant, and the cerium salt solvent is 3-4:6-7:6-7:1.
[0055] In a further preferred embodiment, in step 1, the weight ratio of the acid source, the solvent, the cerium salt and the surfactant is 3.7:6.7:6.7:1.
[0056] In a specific embodiment, in step 1, the reaction conditions include: temperature of 100-250°C, and time of 1-6 h. In a preferred embodiment, in step 1, the reaction conditions include: temperature of 140-180°C, and time of 2-4 h.
[0057] In a further preferred embodiment, the reaction conditions include: temperature of 160° C. and time of 3 h.
[0058] In a specific embodiment, in step 2, the loading method is an equal volume impregnation method or a deposition-precipitation method.
[0059] In a specific embodiment, in step 2, the nickel salt can be any conventionally selected in the art, as long as the purpose of the present invention can be achieved. In a preferred embodiment, the nickel salt can be nickel nitrate or nickel nitrate hexahydrate.
[0060] In the preparation method described above, when step 2 is an equal volume impregnation method, the steps include: S2, mixing the nickel salt solution and the cerium dioxide hollow spheres obtained in step 1, then performing solid-liquid separation and calcining the obtained solid product.
[0061] In a preferred embodiment, S2 comprises the following steps: dissolving nickel salt in a solvent, dripping the obtained solution into the cerium dioxide hollow nanospheres in batches, stirring evenly and filtering, and calcining the obtained solid product to obtain the catalyst.
[0062] Through this preferred embodiment, the method uses hollow cerium dioxide spheres as carriers to avoid thermal sintering of the catalyst in a high-temperature environment. At the same time, the nickel salt solution is loaded onto the hollow cerium dioxide spheres by batch addition, which is beneficial to obtaining a nickel-based hollow cerium dioxide sphere catalyst with a large specific surface area and improving the catalytic activity of the catalyst.
[0063] In a specific embodiment, in S2, the molar ratio of the cerium dioxide hollow spheres to the nickel salt is 1-4:1.
[0064] In a preferred embodiment, in S2, the molar ratio of the cerium dioxide hollow spheres to the nickel salt is 2-4:1.
[0065] In a specific embodiment, in S2, the solvent can be any conventional solvent in the art, as long as the purpose of the present invention can be achieved. In a preferred embodiment, the solvent can be a mixed solution of ultrapure water and ethanol.
[0066] In the preparation method described above, when step 2 is a deposition-precipitation method, it includes the following steps: (2) Mixing the nickel salt solution, the alkali source and the cerium dioxide hollow spheres obtained in step 1 for reaction, then performing solid-liquid separation and calcining the obtained solid product.
[0067] In a specific embodiment, step (2) comprises the following steps: adding cerium dioxide hollow nanospheres to a nickel salt solution, stirring evenly and then dropping an alkali source solution into the solution, separating the solid and the liquid after the reaction is completed, washing and drying the obtained solid product, and then calcining to obtain the catalyst.
[0068] In a specific embodiment, in step (2), the alkali source can be selected from conventional sources in the art, as long as the purpose of the present invention can be achieved. In a preferred embodiment, in step (2), the alkali source can be a sodium hydroxide solution.
[0069] In a specific embodiment, in step (2), the molar ratio of the cerium dioxide hollow spheres, the alkali source and the nickel salt is 1-4:40-60:1. In a preferred embodiment, in step (2), the molar ratio of the cerium dioxide hollow spheres, the alkali source and the nickel salt is 2-3:45-55:1.
[0070] In a preferred embodiment, in step (2), the concentration of the alkali source is 6-8 mol / L.
[0071] In a specific embodiment, in step (2), the reaction conditions include: temperature of 50-120 °C and time of 10-30 h. In a preferred embodiment, the reaction can be carried out in an autoclave.
[0072] In a preferred embodiment, in step (2), the washing is specifically: using ultrapure water and anhydrous ethanol for cross-centrifugation washing 6 times.
[0073] In a preferred embodiment, in step (2), the drying conditions include: a temperature of 60-100°C and a time of 8-16 hours. In a further preferred embodiment, the drying conditions include: a temperature of 80°C and a time of 10-13 hours.
[0074] In a specific embodiment, in step 1 and step 2, the calcination conditions include: temperature of 400-600°C, time of 2-6 h. In a preferred embodiment, in step 1 and step 2, the calcination conditions include: temperature of 500°C, time of 4 h.
[0075] In a specific embodiment, in step 3, the reduction activation is carried out under a reducing atmosphere, and the conditions of the reduction activation include: a temperature of 400-550° C., a time of 1-5 h, and a reducing gas space velocity of 15-25 mL / min.
[0076] In a preferred embodiment, the reduction activation conditions include: temperature of 450-500 °C, time of 2-4 h, and reduction gas space velocity of 20 mL / min. In a preferred embodiment, the reducing atmosphere can be selected from conventional sources in the art, as long as the purpose of the present invention can be achieved. In a further preferred embodiment, the reducing atmosphere is pure hydrogen.
[0077] The third aspect of the present invention provides a nickel-based cerium dioxide hollow sphere catalyst prepared by the method described above.
[0078] A fourth aspect of the present invention provides an application of the nickel-based ceria hollow sphere catalyst described above in low-temperature catalytic carbon dioxide methanation.
[0079] In the present invention, the catalyst can be applied to the catalytic reaction of carbon dioxide methanation. Compared with 300-600 °C in the prior art, the catalyst of the present invention can effectively reduce the temperature required for the catalytic reaction to 250-450 °C. At the same time, the catalyst of the present invention has good catalytic activity and selectivity. In a preferred embodiment, the carbon dioxide conversion rate of the carbon dioxide methanation reaction catalyzed by the catalyst of the present invention can reach 83%, and the methane selectivity can reach 99.4%.
[0080] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.
[0081] In the following examples and comparative examples, unless otherwise specified, the remaining reagents used are commercially available products.
[0082] Example 1 (1) At room temperature, 0.5 g of cerium nitrate hexahydrate and 0.2 g of PVP were dissolved in 15 mL of ethylene glycol. After sufficient stirring, 1 mL of 1 mol / L HCI solution was added to the resulting solution and stirred continuously for 30 minutes. The resulting clear solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 160 °C for 3 hours. After the reactor was cooled to room temperature, it was cross-washed with deionized water and anhydrous ethanol for 3 times. Subsequently, the sample was dried at 60 °C. Finally, the dried sample was calcined in a muffle furnace at 500 °C for 4 h to obtain mesoporous cerium dioxide hollow nanospheres.
[0083] (2) A nickel-based mesoporous ceria nanosphere catalyst was prepared by an equal volume impregnation method: 0.4 g of nickel nitrate hexahydrate was dissolved in 0.2 mL of a mixture of ultrapure water and ethanol, wherein the ratio of ultrapure water to ethanol was 1:4, and then the mixture was dropwise added to 0.5 g of mesoporous ceria nanosphere powder. The nickel nitrate hexahydrate solution and the mesoporous ceria nanosphere powder were stirred thoroughly with a glass rod to uniformly mix the nickel nitrate hexahydrate solution and the mesoporous ceria nanosphere powder. The resulting mixture was then transferred to a muffle furnace and calcined at 500 °C for 4 h to obtain the nickel-based ceria catalyst.
[0084] According to the attached Figure 1 In the XRD spectrum of the catalyst prepared in this example, the diffraction peak position is basically consistent with the NiO diffraction spectrum (JCPDS PDF#71-1179) and the CeO2 diffraction spectrum (JCPDS PDF#34-0394), which shows that the components of the product prepared in this example are nickel oxide and cerium dioxide; according to the attached drawing Figure 2 From the SEM and TEM spectra of the catalyst prepared in this example, it can be seen that the catalyst prepared in this example is a uniform hollow nanosphere structure with a particle size of 80-100 nm, and no thermal sintering or agglomeration occurs.
[0085] Example 2 (1) At room temperature, 0.5 g of cerium nitrate hexahydrate and 0.2 g of PVP were dissolved in 15 mL of ethylene glycol. After sufficient stirring, 1 mL of 1 mol / L HCI solution was added to the resulting solution and stirred continuously for 30 minutes. The resulting clear solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 160 °C for 3 hours. After the reactor was cooled to room temperature, it was cross-washed with deionized water and anhydrous ethanol for 3 times. Subsequently, the sample was dried at 60 °C. Finally, the dried sample was calcined in a muffle furnace at 500 °C for 4 h to obtain mesoporous cerium dioxide hollow nanospheres.
[0086] (2) A nickel-based mesoporous ceria nano-hollow sphere catalyst was prepared by a deposition-precipitation method: 1 g of mesoporous ceria nano-hollow sphere powder was added to 5 mL of 0.6 mol / L nickel nitrate hexahydrate aqueous solution, and after stirring and mixing at room temperature, 20 mL of 7.5 mol / L sodium hydroxide aqueous solution was dropped into the above mixture; the resulting mixture was then transferred to a high-pressure reactor and reacted at 80 °C for 20 h. After the reaction was completed, the reactor was cooled to room temperature, filtered, and the solid product was cross-washed with deionized water and anhydrous ethanol for 6 times, and then the product was dried at 80 °C; the dried product was placed in a muffle furnace and calcined at 500 °C for 4 h to obtain the nickel-based ceria catalyst.
[0087] According to the attached Figure 1 In the XRD spectrum of the catalyst prepared in this example, the diffraction peak position is basically consistent with the NiO diffraction spectrum (JCPDS PDF#71-1179) and the CeO2 diffraction spectrum (JCPDS PDF#34-0394), which shows that the components of the product prepared in this example are nickel oxide and cerium dioxide; according to the attached drawing Figure 2 From the SEM and TEM spectra of the catalyst prepared in this example, it can be seen that the catalyst prepared in this example is a uniform hollow nanosphere structure with a particle size of 80-100 nm, and no thermal sintering or agglomeration occurs.
[0088] Test Example 1 The N2 adsorption characterization test instrument for the catalyst prepared in Examples 1 and 2 is the Autosorb-iQ-AG-MP fully automatic specific surface and pore analyzer (Quantachrome, USA). The specific surface area and pore size data of the catalyst are calculated by the BET method and the BJH method, respectively.
[0089] The results are shown in Table 1.
[0090] Table 1
[0091] As can be seen from Table 1, by adopting the technical solution of the present invention, compared with the prior art, the catalyst prepared by the method has a larger specific surface area and a good pore structure; in a preferred embodiment, the method adopts an equal volume impregnation method to load nickel onto the mesoporous ceria hollow spheres, which can further increase the specific surface area of the prepared catalyst. The specific surface area of the catalyst prepared in Example 1 is as high as 114.6 m 2 / g, and the high specific area catalyst can provide enough active sites to load nickel, making the nickel species dispersed evenly, thereby improving the catalytic activity.
[0092] Application Example 1 The catalytic performance characterization of the catalysts prepared in Examples 1 and 2 specifically includes the following steps: In this application example, the catalytic performance evaluation of CO2 methanation reaction was carried out on a customized fixed-bed continuous flow reactor. First, 0.1 g of the catalyst device quartz tube (id= 8.00 mm) was weighed, and the temperature was raised to 490°C at a heating rate of 1°C / min, and reduced in a pure H2 (20.0 mL / min) environment for 3 h. Subsequently, the CO2 methanation activity test was carried out in the temperature range of 250~450 °C. The test conditions were: 80% H2 / 20% CO2 mixed gas flow rate was 20 mL / min, and the space velocity (WGHSV) was 12000 mL / (g∙h). In addition, the catalyst stability test was carried out at 400 °C for 20 h, and the gas flow rate required for the test was consistent with the activity test. The generated gas was analyzed online using a GC-7900 gas chromatograph (Techcomp, Shanghai) equipped with a thermal conductivity detector (TCD) and a hydrogen fire detector (FID). CO2 conversion rate (denoted as ), CH4 selectivity (denoted as ) is calculated as follows:
[0093] The results are shown in Table 2.
[0094] Table 2
[0095] It can be seen from Table 2 that by adopting the technical solution of the present invention, compared with the prior art, the catalyst prepared by the present invention has excellent catalytic performance and methane selectivity. In a preferred embodiment, the preparation method adopts an equal volume impregnation method, and the prepared catalyst has a carbon dioxide conversion rate of more than 80% and a methane selectivity of more than 98% in the catalytic carbon dioxide methanation reaction.
[0096] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A nickel-based cerium dioxide hollow sphere catalyst, the catalyst comprising cerium dioxide hollow spheres and an active component supported on the hollow spheres; in, The cerium dioxide hollow spheres are mesoporous materials; The active component is nickel oxide and / or metallic nickel; The specific surface area of the catalyst is 80-120 m 2 / g.
2. The catalyst according to claim 1, characterized in that The pore size of the catalyst is 2-10 nm and the pore volume is 0.05-0.5 cm 3 / g.
3. The catalyst according to claim 1 or 2, characterized in that In the catalyst, the molar ratio of nickel element to cerium dioxide is 4-8:
1.
4. A method for preparing a nickel-based cerium dioxide hollow sphere catalyst, characterized in that: The method comprises the following steps: Step 1, mixing a surfactant, a cerium salt, a solvent and an acid source, and then standing to react, then separating the solid and the liquid, and calcining the obtained solid product to obtain cerium dioxide hollow spheres; Step 2, loading nickel salt onto the cerium dioxide hollow spheres obtained in step (1), then performing solid-liquid separation and calcining the obtained solid product; Step 3: Optionally, the product obtained in step 2 is subjected to reduction activation.
5. The method according to claim 4, characterized in that In step 1, the surfactant is polyvinyl pyrrolidone; Preferably, the cerium salt is cerium nitrate; Preferably, the solvent is ethylene glycol; Preferably, the acid source is hydrochloric acid; Preferably, the concentration of the acid source is 0.5-1.5 mol / L; Preferably, the molar ratio of the acid source, the surfactant and the cerium salt solvent is 1-5:4-8:4-8:
1.
6. The method according to claim 4 or 5, characterized in that: In step 1, the reaction conditions include: temperature of 100-250° C., and time of 1-6 h.
7. The method according to any one of claims 4 to 6, characterized in that: In step 2, the loading method is an equal volume impregnation method or a deposition-precipitation method; Preferably, in step 2, the nickel salt is selected from nickel nitrate.
8. The method according to any one of claims 4 to 7, characterized in that: When step 2 is an equal volume impregnation method, it comprises the following steps: S2, mixing the nickel salt solution and the cerium dioxide hollow spheres obtained in step 1 and calcining them.
9. The method according to any one of claims 4 to 8, characterized in that: In S2, the molar ratio of the cerium dioxide hollow spheres to the nickel salt is 1-4:
1.
10. The method according to any one of claims 4 to 7, characterized in that: When step 2 is a deposition-precipitation method, it comprises the following steps: (2) Mixing the nickel salt solution, the alkali source and the cerium dioxide hollow spheres obtained in step 1 for reaction, then performing solid-liquid separation and calcining the obtained solid product.
11. The method according to any one of claims 4 to 7 or 10, characterized in that: In step (2), the alkali source is a sodium hydroxide solution; Preferably, the concentration of the alkali source solution is 6-9 mol / L; Preferably, the concentration of the nickel salt solution is 0.3-1 mol / L; Preferably, in step (2), the molar ratio of the cerium dioxide hollow spheres, the alkali source and the nickel salt is 1-4:40-60:
1.
12. The method according to any one of claims 4 to 7 or 10 and 11, characterized in that: In step (2), the reaction conditions include: temperature of 50-120°C and time of 10-30 h.
13. The method according to any one of claims 4 to 12, characterized in that: In step 1 and step 2, the calcination conditions include: temperature of 400-600° C. and time of 2-6 h.
14. The method according to any one of claims 4 to 13, characterized in that: In step 3, the reduction activation is carried out under a reducing atmosphere, and the conditions of the reduction activation include: a temperature of 400-550° C., a time of 1-5 h, and a reducing gas space velocity of 15-25 mL / min; Preferably, the reducing atmosphere is pure hydrogen.
15. A nickel-based cerium dioxide hollow sphere catalyst prepared by the method described in any one of claims 4 to 14.
16. Use of the nickel-based ceria hollow sphere catalyst according to any one of claims 1 to 3 or the nickel-based ceria hollow sphere catalyst according to claim 15 in catalytic carbon dioxide methanation.
Citation Information
Patent Citations
Nickel-based catalyst for carbon dioxide methanation, preparation method and applications thereof
CN110433815A
Low-temperature high-activity Ni-based catalyst and application thereof
CN113145123A
Cerium dioxide fibrous catalyst containing nickel particles and preparation method thereof
CN113351211A
Preparation method and application of nickel / cerium oxide catalyst
CN114733528A
Reverse Ni / CeO2 catalyst as well as preparation method and application thereof
CN116899568A