Preparation method of BiFeO3 / BiOI heterojunction composite photocatalyst
Through the preparation of BiFeO3/BiOI heterojunction composite photocatalyst, the efficiency limitation problem of BiFeO3 and BiOI in the field of photocatalysis is solved, high absorption of visible light and photogenerated carrier separation are achieved, and photocatalytic efficiency and stability are improved. It has wide application prospects.
Patent Information
- Application Number
- CN202411059579.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-04
- Publication Date
- 2024-11-19
AI Technical Summary
The application of BiFeO3 in the field of photocatalysis is limited by low photogenerating electron-hole separation effect, low conduction band position and small surface area. BiOI alone has the problem of easy decomposition of light and low charge transfer rate caused by narrow bandgap.
BiFeO3/BiOI heterojunction composite photocatalyst is prepared by reacting bismuth salt and iron salt in ethylene glycol and methanol solvent, and BiFeO3 nanocrystals are prepared by heat treatment, and then BiFeO3/BiOI heterojunction composite photo is formed by hydrothermal method. Catalysts to enhance the absorption of visible light and separation of photogenerated carriers.
The photocatalytic efficiency is improved, and the obtained catalyst has high crystallinity, stability and excellent visible photocatalytic activity, and is suitable for photolysis and degradation of organic pollutants.
Smart Images

Figure HDA0004977456560000011 
Figure HDA0004977456560000012 
Figure HDA0004977456560000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic material preparation, in particular to a method for preparing a BiFeO3 / BiOI heterojunction composite photocatalyst. Background Art
[0003] BiFeO3 has a tripartite twisted perovskite structure and is a new multifunctional material that has ferromagnetism at room temperature. Compared with TiO2, which has a wider bandgap, BiFeO3 has a narrow bandgap (2.3eV-3.0eV), which can greatly improve the efficiency of sunlight utilization. In addition, BiFeO3 has good chemical stability and good visible light response characteristics, which makes it have great potential application prospects in the field of photocatalysis. However, due to its low photogenerated electron-hole separation effect, low conduction band position, and small surface area available for catalytic reactions, the photocatalytic efficiency is limited, reducing its effect in practical applications. [4] . With the increase of the atomic number of halogen, the photocatalytic performance of bismuth oxyhalide BiOX continues to increase. Therefore, BiOI is the compound whose photocatalytic performance has been studied the most among bismuth-based catalysts. BiOI is a highly anisotropic layered semiconductor with a narrow energy band gap of (1.7eV-1.9eV) and a wide visible light response range. It can enable photogenerated electrons to quickly migrate to the surface, which is beneficial to improve the separation efficiency of photogenerated electron-hole pairs, thereby improving the photocatalytic activity. Therefore, BiOI is a photocatalyst with excellent photocatalytic degradation performance. However, when BiOI is used alone as a photocatalytic material, BiOI has the disadvantages of being easily decomposed by light and having a low charge transfer rate caused by the narrow band gap.
[0004] Therefore, a new photocatalyst preparation method still needs to be studied to enhance the absorption of visible light, promote the separation of photogenerated carriers, and improve the photocatalytic efficiency. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing a BiFeO3 / BiOI heterojunction composite photocatalyst. The method compounds BiFeO3 and BiOI to form a BiFeO3 / BiOI heterojunction composite photocatalyst, which can enhance the absorption of visible light, promote the separation of photogenerated carriers, and improve the photocatalytic efficiency.
[0006] The present invention solves the above technical problems with the following technical solutions:
[0007] The preparation method of the BiFeO3 / BiOI heterojunction composite photocatalyst of the present invention comprises the following steps:
[0008] S1: Dissolve 1.940-1.261 g of bismuth salt and 1.081-1.616 g of iron salt in 50 ml of a mixture of ethylene glycol and methanol in a volume ratio of 6:4-9, and stir vigorously at 75-80° C. for 3 hours to obtain a mixture for use;
[0009] S2: placing the mixed solution obtained in step S1 in a drying oven and heating it at 120-150° C. until all the liquid evaporates to obtain a powder;
[0010] S3: placing the powder obtained in step S2 in a muffle furnace and calcining it at 350-400°C for 2 hours to remove the organic matter remaining in the reaction, and then placing the powder in a tube furnace and calcining it at 580-600°C for 2 hours to obtain BiFeO3 nanocrystals;
[0011] S4: Weigh 0.2 g of the BiFeO3 nanocrystals prepared in step S3 and dissolve them in 30 ml of deionized water, then add 0.1-0.8 g of bismuth salt, stir and then add an equal amount of KI, continue stirring, and then transfer to a reactor lined with tetrafluoroethylene, place the reactor in a drying oven at 160-180°C to react for 12 hours, cool and centrifuge, wash and dry to obtain a BiFeO3 / BiOI heterojunction composite photocatalyst.
[0012] In step S1 of the present invention, the bismuth salt is bismuth chloride or bismuth nitrate.
[0013] In step S1 of the present invention, the iron salt is ferric chloride or ferric nitrate.
[0014] In step S2 of the present invention, the heating time is 24 to 48 hours.
[0015] In step S4 of the present invention, the washing is performed by washing with deionized water and anhydrous ethanol three times each, and the drying is performed by placing the product in a drying oven at 80° C. and drying it for 24 hours.
[0016] The ethylene glycol and methanol used in the present invention are analytically pure, with a purity of ≥99.5%.
[0017] The bismuth nitrate (Bi(NO3)3·5H2O) of the present invention is analytically pure with a purity of 99.0%.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention selects bismuth salt and iron salt as raw materials, uses ethylene glycol and methanol as solvents, and reacts in a solvent thermal environment to prepare BiFeO3, calcine and crystallize, and then uses a hydrothermal method to prepare the BiFeO3 / BiOI heterojunction composite photocatalyst. The catalyst can enhance the absorption of visible light, promote the separation of photogenerated carriers, and improve the photocatalytic efficiency. In addition, the preparation process is simple, the repeatability is good, and it has great promotion and application value.
[0020] (2) The BiFeO3 / BiOI heterojunction composite photocatalyst obtained by the method of the present invention has high crystallinity, good product morphology and stability, controllable size and uniform size. In addition, the obtained BiFeO3 / BiOI heterojunction composite photocatalyst has excellent visible light catalytic activity and has broad application prospects in the fields of photocatalytic water splitting to produce hydrogen, degradation of organic pollutants, etc.
[0021] (3) The method of the present invention is significantly different from other preparation methods. The present invention uses a mixture of ethylene glycol and methanol as the reaction solvent. The boiling point of ethylene glycol is relatively high, which is 197°C. During the reaction, ethylene glycol and methanol serve as both solvent and reducing agent to prevent Bi 3+ Oxidation to Bi 5+ , so there is no need to add any stabilizer. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the XRD diagram of BiOI and BiFeO3 / BiOI-X of the present invention. Figure 1 Among: (a) BiFeO3 / BiOI-6.25%; (b) BiFeO3 / BiOI-12.5%; (c) BiFeO3 / BiOI-25%; (d) BiFeO3 / BiOI-50%; (e) BiFeO3 / BiOI-75%; (f) pure BiOI.
[0023] Figure 2 The following are scanning electron microscope (SEM) images of BiOI and samples obtained in the present invention. In the images: (a) BiFeO3 / BiOI-6.25%; (b) BiFeO3 / BiOI-12.5%; (c) BiFeO3 / BiOI-25%; (d) BiFeO3 / BiOI-50%; (e) BiFeO3 / BiOI-75%; (f) pure BiOI.
[0024] Figure 3The UV-visible solid diffuse reflectance spectra of BiOI and the samples obtained in the present invention are shown in the figure: (a) BiFeO3 / BiOI-6.25%; (b) BiFeO3 / BiOI-12.5%; (c) BiFeO3 / BiOI-25%; (d) BiFeO3 / BiOI-50%; (e) BiFeO3 / BiOI-75%; (f) pure BiOI.
[0025] Figure 4 The photocatalytic degradation effect of methyl orange by BiOI and the samples of the present invention under visible light irradiation is shown as follows: (a) BiFeO3 / BiOI-6.25%; (b) BiFeO3 / BiOI-12.5%; (c) BiFeO3 / BiOI-25%; (d) BiFeO3 / BiOI-50%; (e) BiFeO3 / BiOI-75%; (f) pure BiOI. DETAILED DESCRIPTION
[0026] The present invention is further described below with reference to specific examples. The experimental methods used in the following examples are all conventional methods unless otherwise specified. The raw materials and auxiliary agents used are all commercially available from conventional markets unless otherwise specified.
[0027] Example 1: The preparation method of BiFeO3 / BiOI heterojunction composite photocatalyst is as follows:
[0028] (1) Weigh Bi(NO3)3.5H2O (1.940 g, 0.004 mol) and Fe(NO3)3.9H2O (1.616 g, 0.004 mol) and dissolve them in a beaker containing 50 ml of a mixed solution of ethylene glycol and methanol (the volume ratio of ethylene glycol to methanol is 6:9). Then stir vigorously at 80°C for 3 hours, and then place the solution in a drying oven and heat it at 120°C for 24 hours to evaporate all the liquid. Then place the obtained powder in a muffle furnace and calcine at 400°C for 2 hours to remove the organic matter remaining in the reaction. Then place the powder in a tube furnace and calcine at 600°C for 2 hours to obtain BiFeO3 nanocrystals.
[0029] (2) 0.20 g of the prepared BiFeO3 nanocrystals were added to 30 ml of deionized water, and then 0.15 g of Bi(NO3)3.5H2O was added. After stirring for 10 minutes, 0.063 g of KI solid was added, and stirring was continued for 10 minutes. Then, the mixture was transferred to a 50 ml tetrafluoroethylene lined reactor, and the reactor was placed in a 160°C drying oven for reaction for 12 hours. After cooling, the reactor was centrifuged and washed with deionized water and anhydrous ethanol three times respectively, and then dried in a drying oven at 80°C for 24 hours to obtain a BiFeO3 / BiOI heterojunction composite photocatalyst. The label is BiFeO3 / BiOI-6.25%.
[0030] By changing the amount of added Bi(NO3)3.5H2O and KI, a series of composite photocatalysts with different mass percentages were obtained, marked as BiFeO3 / BiOI-X (X represents the percentage of BiOI in the composite photocatalyst).
[0031] Example 2 The preparation method of BiFeO3 / BiOI heterojunction composite photocatalyst is as follows:
[0032] (1) Weigh BiCl3 (1.261 g, 0.004 mol) and Fe(NO3)3·9H2O (1.616 g, 0.004 mol) and dissolve them in a beaker containing 50 ml of a mixed solution of ethylene glycol and methanol (the volume ratio of ethylene glycol to methanol is 6:6). Then stir the mixed solution vigorously at 80°C for 3 hours, and then heat the solution at 130°C in a drying oven for 24 hours to evaporate all the liquid. Then place the obtained powder in a muffle furnace and calcine at 350°C for 2 hours to remove the organic matter remaining in the reaction. Then place the powder in a tube furnace and calcine at 600°C for 2 hours to obtain BiFeO3 nanocrystals.
[0033] (2) 0.2 g of the prepared BiFeO3 nanocrystals were added to 30 ml of deionized water, and then 0.15 g of Bi(NO3)3.5H2O was added. After stirring for 10 minutes, 0.063 g of KI solid was added, and stirring was continued for 10 minutes. Then, the mixture was transferred to a 50 ml tetrafluoroethylene lined reactor, and the reactor was placed in a 170°C drying oven for reaction for 12 hours. After cooling, the reactor was centrifuged and then washed with deionized water and anhydrous ethanol three times each, and dried in a drying oven at 80°C for 24 hours to obtain a BiFeO3 / BiOI heterojunction composite photocatalyst. The label is BiFeO3 / BiOI-6.25%.
[0034] By changing the amount of added Bi(NO3)3.5H2O and KI, a series of composite photocatalysts with different mass percentages were obtained, marked as BiFeO3 / BiOI-X (X represents the percentage of BiOI in the composite photocatalyst).
[0035] Example 3 The preparation method of BiFeO3 / BiOI heterojunction composite photocatalyst is as follows:
[0036] (1) Weigh Bi(NO3)3.5H2O (1.940 g, 0.004 mol) and Fe(NO3)3.9H2O (1.616 g, 0.004 mol) and dissolve them in a beaker containing 50 ml of a mixed solution of ethylene glycol and methanol (the volume ratio of ethylene glycol to methanol is 6:4). Then stir the mixed solution vigorously at 75°C for 3 hours, and then heat the solution at 150°C in a drying oven for 36 hours to evaporate all the liquid. Then place the obtained powder in a muffle furnace and calcine at 400°C for 2 hours to remove the organic matter remaining in the reaction. Then place the powder in a tube furnace and calcine at 600°C for 2 hours to obtain BiFeO3 nanocrystals.
[0037] (2) 0.2 g of the prepared BiFeO3 nanocrystals were added to 30 ml of deionized water, and then 0.30 g of Bi(NO3)3.5H2O was added. After stirring for 10 minutes, 0.126 g of KI solid was added and the stirring was continued for 10 minutes. Then the mixture was transferred to a 50 ml tetrafluoroethylene lined reactor. The reactor was placed in a 180°C drying oven for reaction for 12 hours. After cooling, the reactor was centrifuged and washed with deionized water and anhydrous ethanol three times each. The mixture was then placed in a drying oven at 80°C for 24 hours to obtain a BiFeO3 / BiOI heterojunction composite photocatalyst. The catalyst was labeled as BiFeO3 / BiOI-12.5%.
[0038] By changing the amount of added Bi(NO3)3.5H2O and KI, a series of composite photocatalysts with different mass percentages were obtained, marked as BiFeO3 / BiOI-X (X represents the percentage of BiOI in the composite photocatalyst).
[0039] Example 4 The preparation method of BiFeO3 / BiOI heterojunction composite photocatalyst is as follows:
[0040] (1) Weigh Bi(NO3)3.5H2O (1.94 g, 0.004 mol) and FeCl3.6H2O (1.081 g, 0.004 mol) and dissolve them in a beaker containing 50 ml of a mixed solution of ethylene glycol and methanol (the volume ratio of ethylene glycol to methanol is 6:9). Then stir the mixed solution vigorously at 80°C for 3 hours, and then heat the solution at 150°C in a drying oven for 48 hours to evaporate all the liquid. Then place the obtained powder in a muffle furnace and calcine at 400°C for 2 hours to remove the organic matter remaining in the reaction. Then place the powder in a tube furnace and calcine at 580°C for 2 hours to obtain BiFeO3 nanocrystals.
[0041] (2) 0.2 g of the prepared BiFeO3 nanocrystals were added to 30 ml of deionized water, and then 0.60 g of Bi(NO3)3.5H2O was added. After stirring for 10 minutes, 0.252 g of KI solid was added, and stirring was continued for 10 minutes. Then, the mixture was transferred to a 50 ml tetrafluoroethylene lined reactor, and the reactor was placed in a 160°C drying oven for reaction for 12 hours. After cooling, the reactor was centrifuged, and then washed with deionized water and anhydrous ethanol three times each, and then placed in a drying oven at 80°C for 24 hours to obtain a BiFeO3 / BiOI heterojunction composite photocatalyst. The label is BiFeO3 / BiOI-25.0%.
[0042] By changing the amount of added Bi(NO3)3.5H2O and KI, a series of composite photocatalysts with different mass percentages were obtained, marked as BiFeO3 / BiOI-X (X represents the percentage of BiOI in the composite photocatalyst).
[0043] The morphology and structure of the BiFeO3 / BiOI heterojunction composite photocatalyst prepared by the present invention are analyzed as follows:
[0044] The samples obtained in the present invention were tested using a D8 ADVANCE X-ray solid powder diffractometer produced by Bruker, Germany. Figure 1 It can be seen that the XRD pattern of BiOI is almost consistent with the standard pattern (JCPDS NO.40-0548), indicating that the sample has high purity but contains a small amount of impurities, while the diffraction peak intensity of the sample is high and the crystallinity is good. The (012), (110), (004), (020) and (112) crystal planes of BiOI are respectively corresponding to 32.33°, 33.19°, 41.23°, 47.82° and 56.91°. It is reported that the pure phase BiFeO3 crystal is a rhombus-distorted perovskite structure. For the BiFeO3 / BiOI heterojunction composite photocatalyst, as the content of bismuth iodide increases, its weak diffraction peak begins to appear, including both the diffraction peak of BiFeO3 and the diffraction peak of BiOI. The peak intensity of the BiFeO3 / BiOI heterojunction composite photocatalyst is high, proving that the composite material formed by BiFeO3 and BiOI has a good degree of crystallinity. In addition, after doping with different proportions of BiOI, the diffraction peak position of the BiFeO3 / BiOI-X composite material did not change, indicating that the crystal structure of BiFeO3 and BiOI in the BiFeO3 / BiOI composite material did not change.
[0045] Figure 2(a)-(f) are SEM images of the obtained samples. Figure (f) is pure BiOI. It can be seen from the figure that the microscopic morphology of the pure phase BiOI is composed of multiple disordered micron sheets stacked into irregular blocks. It is reported that the microscopic morphology of pure phase BiFeO3 nanoparticles is spherical, and pure phase BiOI nanoparticles aggregate into block particles in a uniform manner. Figures (a)-(e) are to explore the morphology of BiFeO3 / BiOI with different mass fractions of BiOI. From Figure (a) to Figure (e), as the mass fraction of BiOI in the BiFeO3 / BiOI composite material continues to increase, the aggregated block particles of BiOI become larger and more numerous, BiFeO3 is in the form of small spheres attached to the surface of BiOI, and the spherical shape of BiFeO3 and the block structure of BiOI are also dispersed. In this composite catalyst, BiFeO3 and BiOI have a large contact area, which is conducive to the formation of a heterogeneous semiconductor composite structure, expands the spectral visible light response range, and is more conducive to the separation of photogenerated electrons and hole pairs, thereby greatly improving its photocatalytic activity.
[0046] The photocatalytic activity of the BiFeO3 / BiOI heterojunction composite photocatalyst of the present invention was evaluated as follows:
[0047] The photocatalytic activity evaluation reaction was carried out on an XPS-VII type reaction device (produced by Nanjing Xujiang Electromechanical Plant) using a quartz glass reactor with a volume of 200 ml. A 1000W xenon lamp was used as a UV-visible light source, and a self-made filtrate was used to absorb the UV light source to obtain a visible light source. The filtrate used 2M NaNO3 to absorb light with a wavelength below 400nm. The solution layer was located in the interlayer between the lamp tube and the circulating cooling water, so that after further absorbing the UV light through the water layer, the UV light absorption rate reached more than 98%. 20 mg of the BiFeO3 / BiOI heterojunction composite photocatalyst of the present invention was added to 200 ml of methyl orange solution (20 mg / l), first ultrasonically dispersed in a dark room for 15 min to obtain a better dispersion state, and in order to achieve desorption-adsorption equilibrium, before turning on the light, magnetic stirring adsorption was performed for 1 h under the condition of passing 200 ml / min of air, and then the photocatalytic reaction was carried out at room temperature. During the reaction, 8 ml of sample was taken at regular intervals, and the obtained suspension was centrifuged in a high-speed centrifuge for 10 min to remove the catalyst suspended in the solution. The supernatant was taken and its concentration was tested using a Hitachi UV-3010 spectrophotometer.
[0048] The decolorization efficiency of methyl orange can be calculated by X%=(A0-A) / A0×100%, where A0 is the absorbance of 20 mg / l MO at 465 nm, and A is the absorbance of methyl orange samples taken out at different times.
[0049] Depend on Figure 3It can be seen that the main absorption wavelength of BiOI is less than 450nm. The BiFeO3 / BiOI heterojunction composite photocatalyst of the present invention has better absorption characteristics in the visible light region, and the absorption capacity in the 500nm-600nm region is significantly enhanced, the absorption edge can reach 750nm, and it also has good absorption in the ultraviolet region. As the amount of bismuth iodide increases, the visible light absorption intensity of the BiFeO3 / BiOI heterojunction composite photocatalyst of the present invention gradually weakens.
[0050] Under the action of visible light, the photocatalytic degradation effect of the obtained sample on methyl orange is as follows: Figure 4 .Depend on Figure 4 It can be seen that the degradation rate of pure BiOI for methyl orange within 150 minutes is only about 43%, while the degradation rate of methyl orange by the BiFeO3 / BiOI heterojunction composite photocatalyst of the present invention is significantly higher than that of pure BiOI. Among them, BiFeO3 / BiOI-25% has the best photocatalytic effect, and the degradation rate of methyl orange by this material is as high as about 97%. With the increase of the mass fraction of bismuth iodide oxide, the photocatalytic efficiency of the BiFeO3 / BiOI heterojunction composite photocatalyst of the present invention shows a trend of first increasing and then decreasing.
[0051] In summary, the BiFeO3 / BiOI heterojunction photocatalyst formed by BiFeO3 and BiOI has a significant effect on the photocatalytic activity of the sample.
[0052] The BiFeO3 / BiOI heterojunction composite photocatalyst (fading rate 98.7%) of the present invention exhibits an excellent visible light catalytic effect, which shows that the BiFeO3 / BiOI heterojunction composite photocatalyst prepared by the present invention has a good effect of degrading organic pollutants.
Claims
1. A method for preparing a BiFeO3 / BiOI heterojunction composite photocatalyst, characterized in that: The method comprises the following steps: Step S1: dissolving 1.940-1.261 g of bismuth salt and 1.081-1.616 g of iron salt in 50 ml of a mixed solution containing ethylene glycol and methanol in a volume ratio of 6:4-9, and stirring vigorously at 75-80° C. for 3 hours to obtain a mixed solution for use; Step S2: placing the mixed solution obtained in step S1 in a drying oven and heating it at 120-150° C. until all the liquid evaporates to obtain a powder; Step S3: placing the powder obtained in step S2 in a muffle furnace and calcining it at 350-400°C for 2 hours to remove the organic matter remaining in the reaction, and then placing the powder in a tube furnace and calcining it at 580-600°C for 2 hours to obtain BiFeO3 nanocrystals; Step S4: Weigh 0.2 g of the BiFeO3 nanocrystals prepared in step S3 and dissolve them in 30 ml of deionized water, then add 0.1-0.8 g of bismuth salt, stir and then add an equal amount of KI, continue stirring, and then transfer to a reactor lined with tetrafluoroethylene, place the reactor in a drying oven at 160-180°C to react for 12 hours, cool and centrifuge, wash and dry to obtain a BiFeO3 / BiOI heterojunction composite photocatalyst.
2. The method of BiFeO3 / BiOI heterojunction composite photocatalyst according to claim 1, characterized in that: In step S1, the bismuth salt is bismuth chloride or bismuth nitrate.
3. The method of BiFeO3 / BiOI heterojunction composite photocatalyst according to claim 1 or 2, characterized in that: In step S1, the iron salt is ferric chloride or ferric nitrate.
4. The method of BiFeO3 / BiOI heterojunction composite photocatalyst according to claim 1 or 2, characterized in that: In step S2, the heating time is 24 to 48 hours.
5. The method of BiFeO3 / BiOI heterojunction composite photocatalyst according to claim 1 or 2, characterized in that: In step S4, the washing is performed by washing with deionized water and anhydrous ethanol three times each, and the drying is performed by placing the product in a drying oven at 80° C. for 24 hours.