Electret dust collection filter material and preparation method thereof

By using polypropylene, electret polymer, nanosilicate and nanosilicon dioxide composite in electret filter materials, as well as quaternary ammonium ionic liquid and polyethylene wax composite, and laser perforation treatment, the current situation is solved There are problems of electret durability and filtration resistance in the technology, and efficient electret filtration effect and antibacterial performance are achieved.

CN118976597AInactive Publication Date: 2024-11-19ANHUI TONGDA SMART TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411062952.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing electret filter materials cannot obtain long-lasting electret durability, and the small pore size of the filter material leads to an increase in filtration resistance and is prone to clogging.

Method used

Polypropylene, electret polymer, nanosilicate and nanosilicon dioxide composites are used as electret enhancers, combined with quaternary ammonium ionic liquid and polyethylene wax composites as functional enhancers, and a rectangular array is formed through laser perforation. Distribute micropores, prepare hollow plates to improve dust-retaining capacity and efficiency of filter materials.

Benefits of technology

It improves the electret durability and antibacterial properties of the material, reduces filtration resistance, increases the void and surface area of ​​the filter material, and improves filtration efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976597A_ABST
    Figure CN118976597A_ABST
Patent Text Reader

Abstract

The invention is suitable for the technical field of filter materials, and provides an electret dust collection filter material and a preparation method thereof, the electret dust collection filter material comprises the following components by weight: 70-90 parts of polypropylene, 15-25 parts of an electret enhancer, 2-5 parts of a function enhancer, and 3-5 parts of a processing aid; the electret reinforcing agent is an electret polymer, nano silicate and nano silicon dioxide, and the weight ratio of the electret polymer to the nano silicate to the nano silicon dioxide is (2-3): (2-6): (1-2); the electret polymer, the nano silicate and the nano silicon dioxide are compounded to serve as the electret enhancer, the electret durability of the material is improved, the quaternary ammonium salt ionic liquid and the polyethylene wax are compounded to serve as the functional enhancer, an auxiliary electret is formed, the broad-spectrum antibacterial performance can be provided, the antibacterial and bacteriostatic capacity of the material is enhanced, and the service life of the material is prolonged. Meanwhile, the polyethylene wax is used for coating quaternary ammonium salt ions, so that efficient charge capture and release are formed, and the electret effect of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of filter materials, and in particular relates to an electret dust collection filter material and a preparation method thereof. Background Art

[0002] Electret filter material is referred to as electret. It is a type of dielectric material that can store space charge and dipole charge for a long time. It uses the electrostatic effect of the charge to collect dust particles and acts as a low-resistance electrostatic dust filter for air. Compared with traditional filter materials, electret air filter materials have unique dust filtration mechanism, low flow resistance and high efficiency. The electrostatic charging methods of electret mainly include electrostatic spinning, low-temperature plasma discharge, friction charging, thermal polarization and electron beam bombardment. Due to different electrostatic charging methods, the properties of the electret formed are also very different.

[0003] In the prior art, most electret filter materials use tourmaline, barium titanate, and fluorine-containing polymers to increase the electret effect, but long-lasting electret durability cannot be achieved, and the filter material has a small pore size, which easily causes clogging of the filter material and increases the filtration resistance. Therefore, in order to solve the above problems, an electret dust collection filter material and a preparation method thereof are proposed. Summary of the invention

[0004] The invention provides an electret dust collecting filter material and a preparation method thereof, aiming to solve the problem that the electret filter material cannot obtain long-lasting electret durability and the filtering resistance increases.

[0005] The present invention is implemented as follows: an electret dust collection filter material comprises the following components in parts by weight: 70 to 90 parts of polypropylene, 15 to 25 parts of an electret enhancer, 2 to 5 parts of a functional enhancer, and 3 to 5 parts of a processing aid;

[0006] The electret reinforcing agent is an electret polymer, a nano-silicate and a nano-silicon dioxide, and the weight ratio of the electret polymer, the nano-silicate and the nano-silicon dioxide is 2-3:2-6:1-2;

[0007] The electret polymer is one of polyvinylidene fluoride, polyvinylidene fluoride and polyimide.

[0008] Preferably, the functional enhancer is a compound of a quaternary ammonium salt ionic liquid and a polyethylene wax, and the weight ratio of the quaternary ammonium salt ionic liquid to the polyethylene wax is 1:2-5.

[0009] Preferably, the processing aid is an antioxidant and a lubricant, the weight ratio of the antioxidant to the lubricant is 1:1-2, and the antioxidant is a compound of antioxidant A and antioxidant B, the weight ratio of antioxidant A to antioxidant B is 2-3:1-2.

[0010] Preferably, the antioxidant A is one of 4,4'-thiobis(6-tert-butyl-3-methylphenol) and 4,4'-methylenebis(2,6-di-tert-butylphenol).

[0011] Preferably, the antioxidant B is one of tris(2,4-di-tert-butylphenyl)phosphite and 2,4-di(n-octylthiomethylene)-6-methylphenol.

[0012] Preferably, the lubricant is a compound of calcium stearate and silicone, and the weight ratio of calcium stearate to silicone is 1 to 2:1.

[0013] A method for preparing an electret dust collection filter material comprises the following steps:

[0014] Weigh polypropylene, electret enhancer, functional enhancer, and processing aid according to weight, and add them into a high-speed mixer for premixing;

[0015] The mixed polypropylene, electret reinforcing agent, functional additives and processing aids are fed into a twin-screw extruder for melt blending to generate a melt;

[0016] The melt is extruded and pressed into a sheet film with a thickness of 0.1 to 0.5 mm;

[0017] The surface of the sheet film is subjected to laser perforation treatment, and 0.02-0.3 mm micro-holes distributed in a rectangular array are formed on the surface of the sheet film by laser perforation.

[0018] Preferably, the method further comprises preparing a function enhancer, wherein the function enhancer is prepared according to the following method:

[0019] Polyethylene wax is added into toluene, the obtained solution is mixed with quaternary ammonium salt ionic liquid, and the mixture is heated until toluene is separated to obtain a functional enhancer.

[0020] Preferably, the method further comprises pressing and folding the melt after extrusion into a wavy film with a notch size of (2-3)*(3-5) mm, the thickness of the wavy film being 0.1-0.5 mm, and compounding the wavy film with the sheet film into a hollow plate.

[0021] Preferably, the hollow plate is subjected to electret treatment, and uniformly distributed charges are generated in the hollow plate by corona discharge to obtain the filter material, and the filter material is piled and cut.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention uses electret polymer, nano-silicate and nano-silicon dioxide as electret enhancers to improve the electret durability of the material, and uses quaternary ammonium salt ionic liquid and polyethylene wax as functional enhancers to form auxiliary electret, which can not only provide broad-spectrum antibacterial performance and enhance the antibacterial and antibacterial capabilities of the material, but also use polyethylene wax to encapsulate quaternary ammonium salt ions to form efficient charge capture and release, thereby improving the electret effect of the material; and by preparing a sheet film and a wavy film, laser drilling holes on the surface of the sheet film to form micropores distributed in a rectangular array, and thermally bonding the sheet film and the wavy film to form a hollow plate, the voids and surface area in the filter material are effectively increased, the dust holding capacity and the filtration efficiency are improved, and the filtration resistance can be effectively reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the process of the present invention;

[0025] Figure 2 It is a schematic diagram of the hollow body molding in the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0027] See also Figure 1 , the present invention provides a technical solution: an electret dust collection filter material, comprising the following components in parts by weight: 70-90 parts of polypropylene, 15-25 parts of an electret enhancer, 2-5 parts of a functional enhancer, and 3-5 parts of a processing aid;

[0028] The electret enhancer is an electret polymer, a nanosilicate and nano-silicon dioxide, the weight ratio of the electret polymer, the nanosilicate and the nano-silicon dioxide is 2-3:2-6:1-2, the electret polymer is one of polyvinylidene fluoride and polyvinylidene fluoride, the molecular weight of the electret polymer is 10000-15000, and the nanosilicate is one or more combinations of calcium silicate, sodium silicate and aluminum silicate.

[0029] The functional enhancer is a compound of quaternary ammonium salt ionic liquid and polyethylene wax, and the weight ratio of the quaternary ammonium salt ionic liquid and the polyethylene wax is 1:2-5, wherein the carbon chain length of the quaternary ammonium salt is 10-12.

[0030] The processing aid is an antioxidant and a lubricant, the weight ratio of the antioxidant to the lubricant is 1:1-2, the antioxidant is a compound of antioxidant A and antioxidant B, the weight ratio of the antioxidant A to antioxidant B is 2-3:1-2, the antioxidant A is one of 4,4'-thiobis(6-tert-butyl-3-methylphenol) and 4,4'-methylenebis(2,6-di-tert-butylphenol), the antioxidant B is one of tris(2,4-di-tert-butylphenyl)phosphite and 2,4-di(n-octylthiomethylene)-6-methylphenol, and the lubricant is a compound of calcium stearate and silicone, the weight ratio of calcium stearate to silicone is 1-2:1.

[0031] The preparation method of the above-mentioned electret dust collection filter material comprises the following steps:

[0032] 1) Preparing materials: preparing a functional enhancer, taking polyethylene wax and adding it to toluene, mixing the obtained solution with a quaternary ammonium salt ionic liquid, heating it to 120° C., separating the toluene, and obtaining a functional enhancer;

[0033] 2) Premixing: Weigh polypropylene, electret enhancer, functional enhancer, and processing aid by weight, and add them into a high-speed mixer for premixing;

[0034] 3) Drying: The premixed materials are dried with hot air in a blast drying oven at a temperature of 65-90°C for 4-6 hours;

[0035] 4) Melting: The mixed polypropylene, electret reinforcement, functional additives and processing aids are fed into a twin-screw extruder for melt blending to generate a melt, wherein the temperature of the twin-screw extruder is 160-235° C., and the aspect ratio of the screw is 15-20:1;

[0036] 5) Extruding the melt and pressing it into a sheet film with a thickness of 0.1 to 0.5 mm;

[0037] 6) performing laser perforation treatment on the sheet film to form 0.02-0.3 mm micro-holes distributed in a rectangular array on the surface of the sheet film by laser perforation;

[0038] 7) After the melt is extruded, it is pressed and folded into a wavy film with a notch size of (2-3)*(3-5) mm, the thickness of the wavy film is 0.1-0.5 mm, and the wavy film is compounded with the sheet film into a hollow plate;

[0039] Wherein, the wavy film and the sheet film are laminated by thermal bonding;

[0040] 8) The hollow plate is subjected to electret treatment, and a uniform charge is generated in the hollow plate by corona discharge to obtain a filter material, and the filter material is piled and cut;

[0041] The electret voltage is 25-60 kV, the electret distance is 10-15 cm, the electret time is 50-100 s, the electret temperature is 20-25° C., and the humidity is 45%-65%.

[0042] Example 1

[0043] The preparation method of the above-mentioned electret dust collection filter material comprises the following steps:

[0044] 1) Preparing materials: preparing a functional enhancer, taking polyethylene wax and adding it to toluene, mixing the obtained solution with a quaternary ammonium salt ionic liquid, wherein the weight ratio of the polyethylene wax to the quaternary ammonium salt ionic liquid is 1:2, heating to 120° C., separating the toluene, and obtaining a functional enhancer;

[0045] 2) Premixing: Weigh 70 parts of polypropylene, 15 parts of electret enhancer, 2 parts of functional enhancer, and 3 parts of processing aid by weight, and add them into a high-speed mixer for premixing;

[0046] The weight ratio of the electret polymer, nanosilicate and nanosilicon dioxide of the electret enhancer is 2:2:1, the electret polymer is polyvinylidene fluoride with a molecular weight of 15,000, and the nanosilicate is calcium silicate; the weight ratio of the quaternary ammonium salt ionic liquid and the polyethylene wax of the functional enhancer is 1:2; the antioxidant is 4,4'-thiobis(6-tert-butyl-3-methylphenol) and tris(2,4-di-tert-butylphenyl)phosphite compounded in a weight ratio of 2:1, and the lubricant is calcium stearate and silicone compounded in a weight ratio of 1:1;

[0047] 3) Drying: The premixed materials are dried with hot air in a blast drying oven at 65°C for 5 hours;

[0048] 4) Melting: The mixed polypropylene, electret reinforcement, functional additives and processing aids are fed into a twin-screw extruder for melt blending to generate a melt, wherein the temperature of the twin-screw extruder is 160-235° C. and the screw aspect ratio is 20:1;

[0049] Among them, the temperature of zone 1 is 165℃, the temperature of zone 2 is 190℃, the temperature of zone 3 is 210℃, the temperature of zone 4 is 235℃, the temperature of zone 5 is 210℃, the temperature of zone 6 is 185℃, and the temperature of zone 7 is 170℃;

[0050] 5) Extruding the melt and pressing it into a sheet film with a thickness of 0.3 mm;

[0051] 6) performing laser perforation treatment on the sheet film to form 0.02 mm micro-holes distributed in a rectangular array on the surface of the sheet film by laser perforation;

[0052] 7) After the melt is extruded, it is pressed and folded into a corrugated film with a notch size of 2*3 mm, the thickness of the corrugated film is 0.5 mm, and the corrugated film is thermally bonded to the sheet film to form a hollow plate;

[0053] 8) The hollow plate is subjected to electret treatment, and a uniform charge is generated in the hollow plate by corona discharge to obtain a filter material, and the filter material is piled and cut, wherein the electret voltage is 25 kV, the electret distance is 10 cm, the electret time is 100 s, the electret temperature is 25° C., and the humidity is 65%.

[0054] Example 2

[0055] 1) Preparing materials: preparing a functional enhancer, taking polyethylene wax and adding it to toluene, mixing the obtained solution with a quaternary ammonium salt ionic liquid, wherein the weight ratio of the polyethylene wax to the quaternary ammonium salt ionic liquid is 1:5, heating to 110° C., separating the toluene, and obtaining a functional enhancer;

[0056] 2) Premixing: Weigh 90 parts of polypropylene, 25 parts of electret enhancer, 5 parts of functional enhancer, and 5 parts of processing aid by weight, and add them into a high-speed mixer for premixing;

[0057] The weight ratio of the electret polymer, nanosilicate and nanosilicon dioxide of the electret enhancer is 3:6:2, the electret polymer is polyvinylidene fluoride with a molecular weight of 10,000, and the nanosilicate is sodium silicate; the functional enhancer is a quaternary ammonium salt ionic liquid and polyethylene wax compounded in a weight ratio of 1:5; the antioxidant is 4,4'-methylenebis(2,6-di-tert-butylphenol) and 2,4-di(n-octylthiomethylene)-6-methylphenol compounded in a weight ratio of 3:2; the lubricant is a calcium stearate and silicone compounded in a weight ratio of 2:1, calcium stearate and silicone;

[0058] 3) Drying: The premixed materials are dried with hot air in a blast drying oven at 90°C for 6 hours;

[0059] 4) Melting: The mixed polypropylene, electret reinforcement, functional additives and processing aids are fed into a twin-screw extruder for melt blending to generate a melt, wherein the temperature of the twin-screw extruder is 160-235° C. and the screw aspect ratio is 15:1;

[0060] Among them, the temperature of zone 1 is 170℃, the temperature of zone 2 is 190℃, the temperature of zone 3 is 210℃, the temperature of zone 4 is 220℃, the temperature of zone 5 is 235℃, the temperature of zone 6 is 200℃, and the temperature of zone 7 is 175℃;

[0061] 5) Extruding the melt and pressing it into a sheet film with a thickness of 0.2 mm;

[0062] 6) The hollow plate is laser perforated to form 0.3 mm micro-holes distributed in a rectangular array in the hollow plate;

[0063] 7) After the melt is extruded, it is pressed and folded into a corrugated film with a notch size of 2*5 mm, the thickness of the corrugated film is 0.3 mm, and the corrugated film is thermally bonded to the sheet film to form a hollow plate;

[0064] The hollow plate is a laminated composite of several layers of porous films and several layers of sheet films, and the composite method of the porous films and the sheet films is thermal bonding;

[0065] 8) The hollow plate is subjected to electret treatment, and a uniform charge is generated in the hollow plate by corona discharge to obtain a filter material, and the filter material is piled and cut;

[0066] Among them, the electret voltage is 60 kV, the electret distance is 15 cm, the electret time is 50 s, the electret temperature is 25° C., and the humidity is 45%.

[0067] Example 3

[0068] 1) Preparing materials: preparing a functional enhancer, taking polyethylene wax and adding it to toluene, mixing the obtained solution with a quaternary ammonium salt ionic liquid, wherein the weight ratio of the polyethylene wax to the quaternary ammonium salt ionic liquid is 1:3, heating to 120° C., separating the toluene, and obtaining a functional enhancer;

[0069] 2) Premixing: 83 parts of polypropylene, 22 parts of electret enhancer, 3 parts of functional enhancer, and 4 parts of processing aid were weighed by weight and added into a high-speed mixer for premixing;

[0070] The weight ratio of the electret polymer, nanosilicate and nanosilicon dioxide of the electret enhancer is 3:5:2, the electret polymer is polyvinylidene fluoride with a molecular weight of 15,000, and the nanosilicate is calcium silicate; the functional enhancer is a quaternary ammonium salt ionic liquid and polyethylene wax compounded in a weight ratio of 1:3; the antioxidant is 4,4'-thiobis(6-tert-butyl-3-methylphenol) and 2,4-di(n-octylthiomethylene)-6-methylphenol compounded in a weight ratio of 3:1; the lubricant is a calcium stearate and silicone compounded in a weight ratio of 1:1;

[0071] 3) Drying: The premixed materials are dried with hot air in a blast drying oven at 90°C for 4 hours;

[0072] 4) Melting: The mixed polypropylene, electret reinforcement, functional additives and processing aids are fed into a twin-screw extruder for melt blending to generate a melt, wherein the temperature of the twin-screw extruder is 160-235° C. and the screw aspect ratio is 20:1;

[0073] Among them, the temperature of zone 1 is 165℃, the temperature of zone 2 is 180℃, the temperature of zone 3 is 200℃, the temperature of zone 4 is 220℃, the temperature of zone 5 is 235℃, the temperature of zone 6 is 200℃, and the temperature of zone 7 is 170℃;

[0074] 5) Extruding the melt and pressing it into a sheet film with a thickness of 0.5 mm;

[0075] 6) The hollow plate is subjected to laser perforation treatment to form 0.1 mm micro-holes distributed in a rectangular array in the hollow plate by laser perforation;

[0076] 7) After the melt is extruded, it is pressed and folded into a corrugated film with a notch size of 3*5 mm, the thickness of the corrugated film is 0.5 mm, and the corrugated film is thermally bonded to the sheet film to form a hollow plate;

[0077] 8) The hollow plate is subjected to electret treatment, and a uniform charge is generated in the hollow plate by corona discharge to obtain a filter material, and the filter material is piled and cut;

[0078] Among them, the electret voltage is 50 kV, the electret distance is 10 cm, the electret time is 85 s, the electret temperature is 20° C., and the humidity is 50%.

[0079] The filter material prepared in Example 1-3 was cut into samples of size 30*30 cm, and the performance test was carried out with NaCl aerosol particles with a mass median diameter of 0.05-0.2 μm as the medium and a flow rate of 85 L / min. The test results are as follows:

[0080] In Example 1, the filtration resistance is 171.66 Pa and the filtration efficiency is 98.35%;

[0081] In Example 2, the filtration resistance is 110.73 Pa and the filtration efficiency is 99.99%;

[0082] In Example 3, the filtration resistance is 192.30 Pa and the filtration efficiency is 99.26%.

[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An electret dust collection filter material, It is characterized in that The invention comprises the following components in parts by weight: 70 to 90 parts of polypropylene, 15 to 25 parts of an electret enhancer, 2 to 5 parts of a functional enhancer, and 3 to 5 parts of a processing aid; The electret reinforcing agent is an electret polymer, nano silicate and nano silicon dioxide, and the weight ratio of the electret polymer, nano silicate and nano silicon dioxide is 2-3:2-6:1-2.

2. An electret dust collection filter material as claimed in claim 1, Features: The functional enhancer is a compound of quaternary ammonium salt ionic liquid and polyethylene wax, and the weight ratio of the quaternary ammonium salt ionic liquid to the polyethylene wax is 1:2-5.

3. An electret dust collection filter material as claimed in claim 1, Features: The processing aids are antioxidants and lubricants, the weight ratio of the antioxidants to the lubricants is 1:1-2, the antioxidants are a compound of antioxidants A and antioxidants B, the weight ratio of the antioxidants A to antioxidants B is 2-3:1-2.

4. An electret dust collecting filter material as claimed in claim 3, Features: The antioxidant A is one of 4,4'-thiobis(6-tert-butyl-3-methylphenol) and 4,4'-methylenebis(2,6-di-tert-butylphenol).

5. An electret dust collection filter material as claimed in claim 3, Features: The antioxidant B is one of tris(2,4-di-tert-butylphenyl)phosphite and 2,4-di(n-octylthiomethylene)-6-methylphenol.

6. An electret dust collecting filter material as claimed in claim 3, Features: The lubricant is a compound of calcium stearate and silicone, and the weight ratio of calcium stearate to silicone is 1-2:

1.

7. A method for preparing an electret dust collection filter material, It is characterized in that The following steps are involved: Weigh polypropylene, electret enhancer, functional enhancer, and processing aid according to weight, and add them into a high-speed mixer for premixing; The mixed polypropylene, electret reinforcing agent, functional additives and processing aids are fed into a twin-screw extruder for melt blending to generate a melt; The melt is extruded and pressed into a sheet film with a thickness of 0.1 to 0.5 mm; The surface of the sheet film is subjected to laser perforation treatment, and 0.02-0.3 mm micro-holes distributed in a rectangular array are formed on the surface of the sheet film by laser perforation.

8. A method for preparing an electret dust collection filter material as claimed in claim 7, It is characterized in that The invention also includes preparing a functional enhancer, wherein the functional enhancer is prepared according to the following method: Polyethylene wax is added into toluene, the obtained solution is mixed with quaternary ammonium salt ionic liquid, and the mixture is heated until toluene is separated to obtain a functional enhancer.

9. A method for preparing an electret dust collection filter material according to claim 7, Features: The method also includes pressing and folding the melt after extrusion into a corrugated film with a notch size of (2-3)*(3-5) mm, a thickness of 0.1-0.5 mm, and compounding the corrugated film with a sheet film into a hollow plate.

10. A method for preparing an electret dust collection filter material according to claim 9, Features: The hollow plate is subjected to electret treatment, and uniformly distributed charges are generated in the hollow plate through corona discharge to obtain filter materials, which are then piled and cut.

Citation Information

Patent Citations

  • Filter

    CN105682770A

  • Melting-expanded electret antibacterial master batch and processing technology and application thereof

    CN111423660A

  • Organic electret material for melt-blown non-woven fabric

    CN112323259A

  • Antibacterial and antiviral melt-blown fabric and preparation method thereof

    CN112921502A

  • Electret master batch composition, electret master batch material, melt-blown cloth and preparation method and application of electret master batch material and melt-blown cloth