Method for directionally preparing strong-light-emitting blocky crystalline silver nano-cluster aggregate
By using chiral D-penicillamine or L-penicillamine as stabilizers at room temperature, silver nanocluster aggregates were formed by adding silver nitrate solution dropwise to form silver nanocluster aggregates, which solved the low luminescence quantum yield and difficult to determine the purity of metal nanoclusters. Problem, the preparation of silver nanocluster aggregates with high purity and high luminescent quantum has been achieved, and has broad application prospects.
Patent Information
- Application Number
- CN202411062575.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The existing metal nanoclusters have low luminescence quantum yields, and it is difficult to construct nanocluster aggregates with high purity and good crystallinity, and the lack of single crystal structure for accurate characterization.
Chiral D-penicillamine or L-penicillamine as stabilizers were used as a stabilizer to prepare strongly luminescent block crystal silver nanocluster aggregates by one-step method, and the directional aggregates were formed by adding silver nitrate solution dropwise and stirring. , and powdery substances are obtained by freeze-drying to achieve high absolute luminescent quantum yield.
It has achieved an absolute luminescent quantum yield of up to 57.7%, with high purity and crystallinity, and is suitable for bioimaging, chemical sensing, bactericidal, catalysis and information encryption.
Smart Images

Figure CN118976896A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for directionally preparing strongly luminescent bulk crystal silver nano cluster aggregates, belonging to the technical field of luminescent nano materials. Background Art
[0002] Metal nanoclusters are nanoclusters composed of a few to hundreds of metal atoms. Their size is similar to the Fermi wavelength of electrons, so they show molecular-like behavior (Kong L, Chu X, Wang C, Zhou H, Wu Y, Liu WD-Penicillamine-coated Cu / Ag alloy nanocluster superstructures: aggregation-induced emission and tunable photoluminescence from red to orange, Nanoscale, 2018, 10, 1631–1640). Due to the presence of metal-metal interactions, metal nanoclusters usually show luminescence behavior. However, the luminescence of metal nanoclusters is usually weak, and the luminescence quantum yield is generally below 1% (Wang S, Meng X, Das A, LiT, Song Y, Cao T, Zhu X, Zhu M, Jin R. A200-fold quantum yield boost in the photoluminescence of silver-doped Ag x Au 25–xnanoclusters:the 13th silver atommatters,Angew.Chem.Int.Ed.2014,53,2376–2380). In recent years, some metal nanoclusters with high luminescence quantum yield have been synthesized, but the highest one generally does not exceed 10% (Shi L, Zhu L, Guo J, Zhang L, Shi Y, Zhang Y, Hou K, Zheng Y, Zhu Y, Lv J, Liu S, Tang Z. Self-assembly of chiral gold clusters into crystalline nanocubes of exceptional optical activity,Angew.Chem.Int.Ed.2017,129,15599–15603). Only some metal nanoclusters that utilize the thermally activated delayed fluorescence mechanism can have a luminescence quantum yield greater than 50% (Han Z, Dong XY, Luo P, Li S, Wang ZY, Zang SQ, Mak TC W. Ultrastable atomically precise chiral silver clusters with more than 95%quantum efficiency, Science Adv. 2020, 6, eaay0107). There are almost no reports on other studies that achieve such high luminescence performance by reducing non-radiative transition strategies (such as aggregation).
[0003] Metal nanoclusters with good crystallinity have attracted wide attention. These nanoclusters usually have properties that other nanoclusters do not have, such as luminescence enhancement caused by crystallization (Chen Y, Li JL, Tong GSM, Lu W, Fu WF, Lai SW, Che CM. Nanostructures of tetranuclear copper(I) complexes with short Cu(I)···Cu(I) contacts: crystallization-induced emission enhancement, Chem. Sci. 2011, 2, 1509–1514). However, there are many isomers of metal nanoclusters, and how to construct metal nanocluster aggregates with high purity and good crystallinity is a great challenge. Although people have tried to construct some nanocluster aggregates with good crystallinity, these aggregates lack single crystal structure and the purity of the nanocluster aggregates cannot be accurately determined by other characterizations (Jia X, Li J, Wang E. Supramolecular self-assembly of morphologydependent luminescent Ag nanoclusters, Chem. Commun. 2014, 50, 9565–9568).
[0004] Based on the above considerations, we used chiral D-penicillamine or L-penicillamine as stabilizers to prepare strong luminescent bulk crystalline silver nanocluster aggregates at room temperature in a "one-step method", with an absolute luminescence quantum yield of up to 57.7%, and characterized them using single crystal structures. As far as we know, we are the first to successfully construct silver nanocluster aggregates with such a high luminescence quantum yield by aggregation. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a method for directional preparation of strongly luminescent bulk crystalline silver nanocluster aggregates. The synthesis method is simple, the yield is high, the cost is low, and a large amount of preparation can be carried out. It has good application prospects in biological imaging, chemical sensing, sterilization, catalysis and information encryption.
[0006] The technical solution of the present invention is a method for directional preparation of strongly luminescent bulk crystalline silver nanocluster aggregates, which is characterized by:
[0007] S1, dissolving a stabilizer in double distilled water to obtain a stabilizer solution; dissolving silver nitrate in double distilled water to obtain a silver nitrate solution;
[0008] S2. Add the silver nitrate solution prepared in S1 dropwise into the stabilizer solution, and stir at room temperature for several days to obtain silver nanocluster aggregates with directional preparation and strong luminescence block crystals.
[0009] Furthermore, the concentration of the stabilizer in S1 is 66-100 mg / mL; the concentration of the silver nitrate solution is 48-62 mg / mL.
[0010] Furthermore, the volume of the stabilizer solution in S1 is 3 mL; the volume of the silver nitrate solution is 1 mL.
[0011] Furthermore, the molar ratio of the stabilizer in S1 to silver nitrate is 3.64 to 7.12:1.
[0012] Furthermore, the stabilizer in S1 is chiral D-penicillamine or L-penicillamine.
[0013] Furthermore, the stirring time in S2 is 3 to 5 days.
[0014] Furthermore, after S2 is stirred, the solution is centrifuged at a speed of 8000-12000 r / min, and after removing the supernatant, the solution is freeze-dried to obtain powdered silver nanocluster aggregates.
[0015] Furthermore, the prepared silver nanocluster aggregates emit strong green light under the irradiation of a portable ultraviolet lamp, and the absolute luminescence quantum yield is as high as 57.7%.
[0016] The beneficial effects of the present invention are as follows: the present invention can directionally prepare strongly luminescent bulk crystalline silver nanocluster aggregates at room temperature through a "one-step method", the synthesis method is simple, and the yield is high and the cost is low, and a large amount of preparation can be carried out. The prepared silver nanocluster aggregates have high purity and good crystallinity, and have good application prospects in biological imaging, chemical sensing, sterilization, catalysis and information encryption.
[0017] The equipment and preparation method adopted by the present invention are very simple. The preparation method of the strongly luminescent bulk crystalline silver nanocluster aggregate provides a good model for the directional design and synthesis of strongly luminescent bulk luminescent materials, and has important guiding and reference significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 : D-penicillamine and the strongly luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 Infrared spectrum.
[0019] Figure 2 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 single crystal structure.
[0020] Figure 3: Strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Examples 1-3 绿 Powder X-ray diffraction of and simulated powder X-ray diffraction pattern based on single crystal results.
[0021] Figure 4-a : Silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectroscopy C1s.
[0022] Figure 4-b : Silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectroscopy of N1s.
[0023] Figure 4-c : Silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectrum O1s.
[0024] Figure 4-d : Silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectroscopy S2p.
[0025] Figure 4-e : Silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectroscopy of Ag 3d.
[0026] Figure 5a : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 Scanning electron microscope photograph.
[0027] Figure 5b : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 2 绿 Scanning electron microscope photograph.
[0028] Figure 5c : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 3 绿 Scanning electron microscope photograph.
[0029] Figure 6 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 Transmission electron microscope photograph of .
[0030] Figure 7 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 The absorption spectrum of .
[0031] Figure 8 : Strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Examples 1-3 绿 luminescence spectrum.
[0032] Fig. 9 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 Glowing photos.
[0033] Fig.10 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 luminescence lifetime. DETAILED DESCRIPTION
[0034] The following embodiments describe the present invention in more detail, but the embodiments do not limit the present invention.
[0035] Example 1 Strong luminescent bulk crystalline silver nanocluster aggregate D 绿 Preparation method (the molar ratio of D-penicillamine to silver nitrate is 3.64)
[0036] S1. Dissolve D-penicillamine (198 mg) in 3 mL of double distilled water and dissolve silver nitrate (62 mg) in 1 mL of double distilled water.
[0037] S2, adding the silver nitrate solution dropwise to the D-penicillamine solution and stirring at room temperature for 4 days to obtain a strongly luminescent block-shaped crystalline silver nanocluster aggregate. The block-shaped crystalline silver nanocluster aggregate powder is centrifuged at a speed of 10000 r / min, the supernatant is removed, and then freeze-dried to obtain.
[0038] Example 2 Strong luminescent bulk crystalline silver nanocluster aggregate D 绿 Preparation method (the molar ratio of D-penicillamine to silver nitrate is 4.88)
[0039] S1. Dissolve D-penicillamine (240 mg) in 3 mL of double distilled water and dissolve silver nitrate (56 mg) in 1 mL of double distilled water.
[0040] S2, adding the silver nitrate solution dropwise to the D-penicillamine solution and stirring at room temperature for 4 days to obtain a strongly luminescent block-shaped crystalline silver nanocluster aggregate. The block-shaped crystalline silver nanocluster aggregate powder is centrifuged at a speed of 10000 r / min, the supernatant is removed, and then freeze-dried to obtain.
[0041] Example 3 Strong luminescent bulk crystalline silver nanocluster aggregate D 绿 Preparation method (the molar ratio of D-penicillamine to silver nitrate is 7.12)
[0042] S1. Dissolve D-penicillamine (300 mg) in 3 mL of double distilled water and dissolve silver nitrate (48 mg) in 1 mL of double distilled water.
[0043] S2, adding the silver nitrate solution dropwise to the D-penicillamine solution and stirring at room temperature for 4 days to obtain a strongly luminescent block-shaped crystalline silver nanocluster aggregate. The block-shaped crystalline silver nanocluster aggregate powder is centrifuged at a speed of 10000 r / min, the supernatant is removed, and then freeze-dried to obtain.
[0044] The strongly luminescent bulk crystalline silver nanocluster aggregates obtained in Examples 1-3 were subjected to infrared light, single crystal, powder X-ray diffraction and simulated X-ray diffraction, scanning electron microscopy, transmission electron microscopy, solid ultraviolet, luminescence spectrum, and luminescence lifetime detection. The specific detection results are as follows.
[0045] Figure 1 The silver nanocluster aggregate D prepared in Example 1 is a strong luminescent bulk crystal. 绿 Infrared spectrum of . It can be seen from the figure that the –1 The infrared spectrum transmission peak has disappeared in the silver nanocluster aggregates, indicating that the S–H bond has been broken and the S–Ag bond has been formed during the formation of the silver nanocluster aggregates.
[0046] Figure 2 The silver nanocluster aggregate D prepared in Example 1 is a strong luminescent bulk crystal. 绿 From the single crystal results, it can be seen that the basic structural unit of silver nanocluster aggregates is Ag5(DPA)6, and there are ligands surrounding them, which is an important reason why silver nanocluster aggregates maintain rigidity.
[0047] Figure 3 The silver nanocluster aggregate D prepared in Example 1-3 with strong luminescence block crystal 绿 Powder X-ray diffraction and simulated powder X-ray diffraction pattern diagram based on single crystal results. It can be seen from the powder X-ray diffraction in Examples 1-3 and the X-ray diffraction pattern simulated by the single crystal that their diffraction peaks are completely consistent, indicating that the silver nanocluster aggregates have a high purity and its powder structure is the same as the single crystal structure.
[0048] Figure 4-a The silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectrum C1s.
[0049] Figure 4-b The silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectrum of N1s.
[0050] Figure 4-c The silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectrum O1s.
[0051] Figure 4-d The silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectrum S2p.
[0052] Figure 4-e The silver nanocluster aggregate D prepared in Example 1 绿 X-ray photoelectron spectrum of Ag3d.
[0053] Figure 4 (ae) shows the X-ray photoelectron spectrum of the silver nanocluster aggregates. As can be seen from the figure, the X-ray photoelectron spectrum of C 1s can be divided into four spectral lines, with peaks at 284.7, 285.5, 286.4, and 288.4 eV, respectively assigned to -CH3, -CS(CH3)2, -CH-, and -CO-. The X-ray photoelectron spectrum of N 1s can be divided into two spectral lines: 401.6 and 406.9 eV, which are assigned to -NH- and -NH3 + The X-ray photoelectron spectrum of O 1s can be divided into two spectral lines, located at 531.3 and 532.7 eV respectively. The X-ray photoelectron spectrum of S2p is divided into two peaks: 162.0 and 163.4 eV, which are assigned to the photoelectron spectra of Ag–S and S–H respectively. The X-ray photoelectron spectrum of Ag 3d is located at 368.7 and 374.7 eV, indicating that the silver element is +1 valence.
[0054] Figure 5a The silver nanocluster aggregate D prepared in Example 1 is a strong luminescent bulk crystal. 绿 Scanning electron microscope photograph.
[0055] Figure 5b The silver nanocluster aggregate D prepared in Example 2 is a strong luminescent bulk crystal. 绿 Scanning electron microscope photograph.
[0056] Figure 5c The silver nanocluster aggregate D prepared in Example 3 is a strong luminescent bulk crystal. 绿 Scanning electron microscope photograph.
[0057] From the scanning electron microscopy ( Figure 5a-5c ) It can be seen that the silver nanocluster aggregates are block-like structures with a size of about 2 μm.
[0058] Figure 6 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 Transmission electron microscope photograph of .
[0059] It can be seen from the transmission electron microscopy image that the silver nanocluster aggregates are block-like structures with a size of about 2μm, which is consistent with the results of the scanning electron microscope.
[0060] Figure 7 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 The absorption spectrum of .
[0061] From the absorption spectrum, it can be seen that the maximum absorption peak of the silver nanocluster aggregates is at 361 nanometers, and the absorption edge is at 400 nanometers. There is no plasma absorption of silver nanoparticles, indicating that the aggregates are composed of silver nanoclusters, which is consistent with the single crystal results.
[0062] Figure 8 : Strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Examples 1-3 绿 From the luminescence spectrum, it can be seen that the silver nanocluster aggregates prepared in Examples 1-3 have the same luminescence spectrum, the maximum luminescence peaks are all located at 548 nanometers, and the luminescence is very strong.
[0063] Fig. 9 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 As can be seen from the figure, D 绿 Exhibits a strong green luminescence.
[0064] Fig.10 : The strong luminescent bulk crystalline silver nanocluster aggregate D prepared in Example 1 绿 The luminescence lifetime of the silver nanocluster aggregates is 3.77 microseconds. Therefore, the luminescence originates from the charge transfer transition from the triplet ligand to the metal-metal ( 3 LMMCT).
[0065] The above embodiments are only used to illustrate the design ideas and features of the present invention, and their purpose is to enable those skilled in the art to understand the content of the present invention and implement it accordingly. The protection scope of the present invention is not limited to the above embodiments. Therefore, any equivalent changes or modifications made based on the principles and design ideas disclosed by the present invention are within the protection scope of the present invention.
Claims
1. A method for directional preparation of strongly luminescent bulk crystalline silver nanocluster aggregates, Its characteristics are: S1, dissolving a stabilizer in double distilled water to obtain a stabilizer solution; dissolving silver nitrate in double distilled water to obtain a silver nitrate solution; S2. Add the silver nitrate solution prepared in S1 dropwise into the stabilizer solution, and stir at room temperature for several days to obtain silver nanocluster aggregates with directional preparation and strong luminescence block crystals.
2. The method for preparing the silver nanocluster aggregates with directional strong luminescence block crystals as claimed in claim 1, Its characteristics are: The concentration of the stabilizer in S1 is 66-100 mg / mL; the concentration of the silver nitrate solution is 48-62 mg / mL.
3. The method for preparing the silver nanocluster aggregates with directional strong luminescence block crystals as claimed in claim 2, Its characteristics are: The molar ratio of the stabilizer in S1 to silver nitrate is 3.64 to 7.12:
1.
4. The method for directional preparation of strongly luminescent bulk crystalline silver nanocluster aggregates as claimed in claim 1, Its characteristics are: S1 The stabilizer is chiral D-penicillamine or L-penicillamine.
5. The method for directional preparation of strongly luminescent bulk crystalline silver nanocluster aggregates as claimed in claim 1, Its characteristics are: The stirring time in S2 is 3 to 5 days.
6. The method for directional preparation of strongly luminescent bulk crystalline silver nanocluster aggregates as claimed in claim 1, Its characteristics are: After S2 is stirred, the solution is centrifuged at a speed of 8000-12000 r / min, and after removing the supernatant, the solution is freeze-dried to obtain powdered silver nanocluster aggregates.
7. The method for directional preparation of strongly luminescent bulk crystalline silver nanocluster aggregates as claimed in claim 1, Its characteristics are: The prepared silver nanocluster aggregates emit strong green light under the irradiation of a portable ultraviolet lamp, and the absolute luminescence quantum yield is as high as 57.7%.