Application of flux-cored wire for Q345qD steel in steel bridge U-rib upward inner welding
By using flux-core welding wire with specific chemical composition and proportional proportions in the Q345qD steel bridge U rib up inner welding, welding defects and splash problems are solved, high-quality welding products are achieved, high-strength level engineering requirements are met, and the improvement of the improvement of Welding efficiency and safety and economicality of bridge structure.
Patent Information
- Application Number
- CN202411106871.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Existing flux-core welding wires are difficult to form high-quality welds in the inner welding of the U-rib up position of the Q345qD steel bridge, and are prone to welding defects and splashes, and are difficult to meet the engineering requirements of high-strength grades.
The chemical composition is used to include 0.035%≤C≤0.06%, 0.4%≤Si≤0.61%, 1.29%≤Mn≤1.6%, S≤0.0085%, and P≤0.017 flux-core welding wire, and TiO2, SiO2, Al2O3, NaF, magnesium powder, manganese metal, silicon manganese alloy and other components, through specific proportional ratios and welding processes, ensure that the melting point is within the range of 990-2050℃. The outer skin of the welding wire is made of low-carbon steel material, with a filling rate of 13.5. ~15.0%.
The formed welded metal has high tensile strength, yield strength and elongation after break. The welding is neatly formed, reducing defects, improving welding quality and efficiency, reducing engineering costs, and improving the safety and economicality of the bridge structure.
Smart Images

Figure CN118977012A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of welding, and particularly relates to application of flux-cored welding wire for Q345qD steel in upward position internal welding of U-ribs of steel bridges. Background Art
[0002] As we all know, in actual welding scenarios, the selection of welding materials must be closely matched with their parent materials.
[0003] Flux-cored welding wires used for low-strength steel (such as Q345qD) are usually mainly used to improve the plasticity and toughness of the weld metal, so as to meet the welding requirements of low-strength steel. Flux-cored welding wires used for high-strength steel need to obtain higher strength and hardness. Therefore, if the flux-cored welding wires used for high-strength steel that are currently disclosed are used to weld low-strength steel, the plasticity and toughness of the weld metal may be insufficient, thereby affecting the quality and performance of the welded joint.
[0004] In addition, different types of steel also have differences in chemical composition, mechanical properties, heat treatment process, etc., so it is necessary to select suitable flux-cored welding wire to meet specific welding requirements. If an unsuitable welding wire is used, it may cause metallurgical incompatibility between the weld metal and its parent material, thus affecting the performance and quality of the welded joint.
[0005] Q345 steel is a high-quality low-alloy structural steel. Due to its good strength and toughness, it is often used in the manufacture of steel structure bridges and other projects that require earthquake resistance. Q345 steel includes models such as Q345qC, Q345qD, and Q345qE. These models of bridge steel plates are thick steel plates used to manufacture bridge structural parts, mainly used to build railways, highway bridges, and cross-sea bridges.
[0006] Among them, Q345qD steel plate has good welding performance and low notch sensitivity, which makes it widely used in bridge construction. It can not only bear the weight of the bridge structure and external loads, but also transmit these forces to the supporting structure of the bridge. At the same time, Q345qD steel also has good durability and stability, and can resist the influence of various natural factors such as wind, rain, temperature changes, etc.
[0007] In general, steel bridges built with Q345qD steel have excellent mechanical properties and stability, and can meet the requirements of modern bridge engineering for safety, stability and economy. Nowadays, Q345qD steel is the most widely used steel plate for building railway or highway bridges.
[0008] Due to the limitation of past technology, the inner side of the U-rib of the built steel bridge has not been internally welded, which results in the cracks that originate from the weld root to the top plate being not only hidden but also difficult to repair. If internal weld treatment is applied to it, the fatigue performance of the bridge deck in service can be improved. By using the internal welding robot of the in-service bridge to enter the interior of the U-rib of the built steel bridge and perform additional internal weld construction in the upper position to form double-sided welds, the fatigue durability of the bridge surface system can be extended.
[0009] In terms of welding, the Q345qD steel bridge internal welding work requires the use of appropriate welding materials and processes to ensure the quality and performance of the weld. Although flux-cored wire is a commonly used welding material, the existing flux-cored wire on the market is very difficult to weld in the overhead welding position because the molten pool formed during the welding process deforms and falls under the action of gravity. It is easy to have problems such as poor weld formation and welding defects. In addition, it is easy to generate more spatter during welding, making it difficult to ensure the welding quality of the Q345qD steel bridge internal welding. Summary of the invention
[0010] In view of the deficiencies in the prior art, the present invention provides an application of a flux-cored welding wire for Q345qD steel in the upward position internal welding of a U-rib of a steel bridge.
[0011] The invention provides application of flux-cored welding wire for Q345qD steel in upward internal welding of U-rib of steel bridge. The chemical components in the flux-cored welding wire include, by mass percentage: 0.035%≤C≤0.06%, 0.4%≤Si≤0.61%, 1.29%≤Mn≤1.6%, S≤0.0085%, P≤0.017, and the balance is Fe.
[0012] Furthermore, the flux-cored welding wire contains TiO 2 、SiO 2 、Al 2 O 3 , NaF, and TiO 2 、SiO 2 、Al 2 O 3 The specific mass ratio of NaF is 36-40:3.5-5.5:1.0-1.6:0.98-2.94. During the welding process, the melting point is maintained in the range of 990-2050℃.
[0013] Furthermore, the flux-cored welding wire also contains magnesium powder, metallic manganese, and silicon-manganese alloy, and the specific mass ratio of magnesium powder, metallic manganese, and silicon-manganese alloy is 3-5:2-4:18-22, and desulfurization and deoxidation reactions are carried out in the early, middle, and late stages of the welding process respectively.
[0014] Furthermore, the mass ratio of silicon to manganese in the silicon-manganese alloy is 17:65.
[0015] Furthermore, the flux-cored welding wire includes a flux core material for the welding wire and a welding wire sheath.
[0016] Furthermore, the welding wire flux core material is filled in the welding wire sheath at a filling rate of 13.5-15.0%.
[0017] Furthermore, the flux core material for welding wire includes the following components in percentage by mass: 38-42% rutile, 5-8% feldspar, 1-3% sodium fluoride, 18-22% silicon manganese alloy, 2-4% metallic manganese, 3-6% magnesium powder, and iron powder is supplemented to 100%.
[0018] Furthermore, the outer sheath of the welding wire is made of low carbon steel material or low alloy steel material.
[0019] Furthermore, the diameter of the flux-cored welding wire is 1.2 mm to 1.4 mm.
[0020] Furthermore, the preparation method of the flux-cored welding wire comprises the following steps:
[0021] 1) Drying the components of the flux core material for welding wire for the first time, adding them into a powder mixer and stirring and mixing them evenly, and then drying the evenly mixed flux core material for welding wire for the second time to obtain a dry powder mixture of the flux core material for welding wire;
[0022] 2) Roll the steel strip used as the outer skin of the welding wire into a U-shaped groove;
[0023] 3) Filling the dry powder mixture of the welding wire core material into the U-shaped groove;
[0024] 4) The U-shaped groove containing the dry powder mixture of the flux core material is closed and rolled into an O-shape, and then drawn to the set diameter of the welding wire.
[0025] Compared with the prior art, the present invention has the following advantages and effects:
[0026] The invention discloses an application of flux-cored welding wire for Q345qD steel in U-rib upward internal welding of steel bridges, wherein the chemical composition of the flux-cored welding wire includes, by mass percentage: 0.035%≤C≤0.06%, 0.4%≤Si≤0.61%, 1.29%≤Mn≤1.6%, S≤0.0085%, P≤0.017, and the remainder is Fe. While meeting the engineering use requirements of high-strength grade steel plates, it can meet the requirements of all-position welding of Q345qD steel, and is particularly suitable for the U-rib upward internal welding engineering of Q345qD steel bridges. The deposited metal formed by the flux-cored welding wire for Q345qD steel provided by the invention after U-rib upward internal welding has the following characteristics: tensile strength ≥545Mpa, yield strength ≥450Mpa, elongation after fracture ≥24%, and absorbed energy ≥34KV at -20°C. 2 / J. The slag formed by the flux-cored welding wire for Q345qD steel in the upward position internal welding of the U-rib of the steel bridge has high viscosity and high toughness, the weld formed by welding is neatly formed, defects are reduced, and spatter is not easy to be generated during welding, which not only ensures the welding quality of the upward position internal welding of the Q345qD steel bridge, but also further improves the welding quality and efficiency of the bridge structure, reduces the engineering cost, and improves the safety and economy of the overall engineering.
[0027] The flux-cored welding wire for Q345qD steel provided by the present invention is mainly used for Q345qD steel, especially for the welding scene of the upward internal welding. Based on the characteristics that Q345qD steel has a relatively low strength level and is a popular bridge steel, compared with the existing flux-cored welding wire, the flux-cored welding wire for Q345qD steel provided by the present invention preferably contains quartz, ferrotitanium, ferroboron and other components, and the standard of the required performance can be achieved through the reasonable proportion of the flux-cored components in the formula. The flux-cored welding wire for Q345qD steel has a small number of components, so that the performance stability of the components mixed in the proportion is good, the manufacturing process of the welding wire is relatively simple, and the relative cost is low, which is conducive to the promotion and application of the product; at the same time, by increasing the amount of iron powder in the flux-cored welding wire for Q345qD steel, the iron content of the transition to the weld is increased, thereby improving the deposition efficiency of the flux-cored welding wire for Q345qD steel, increasing the fullness of the weld of the upward internal welding, and enhancing the welding performance of the flux-cored welding wire for Q345qD steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a weld bead forming diagram of the flux-cored welding wire for Q345qD steel obtained in Example 1; DETAILED DESCRIPTION
[0029] Reference will now be made in detail to various embodiments of the present invention, examples of which are illustrated in the accompanying drawings and described below. Although the present invention will be described in conjunction with exemplary embodiments of the present invention, it should be understood that this specification is not intended to limit the present invention to those exemplary embodiments. On the other hand, the present invention is intended to cover not only the exemplary embodiments of the present invention, but also various alternatives, modifiers, equivalents and other embodiments, which may be included in the spirit and scope of the present invention as defined by the appended claims.
[0030] Hereinafter, exemplary embodiments of the present invention will be described in detail with reference to the accompanying drawings. The specific structures and functions described in the exemplary embodiments of the present invention are for illustrative purposes only. Embodiments according to the concepts of the present invention can be implemented in various forms, and it should be understood that they should not be interpreted as being limited to the exemplary embodiments described in the exemplary embodiments, but include all modifications, equivalents or substitutes included in the spirit and scope of the present invention.
[0031] Throughout the specification, the professional terms used herein are only for describing various exemplary embodiments and are not intended to be limiting. It will be further understood that the terms "include", "comprising", "having", etc., when used in the exemplary embodiments, specifically refer to the presence of the stated parts, steps, operations or elements, but do not exclude the presence or addition of one or more other parts, steps, operations or elements.
[0032] A specific embodiment of the present invention provides an application of a flux-cored welding wire for Q345qD steel in the upward internal welding of a U-rib of a steel bridge, wherein the chemical composition of the flux-cored welding wire includes, by mass percentage: 0.035%≤C≤0.06%, 0.4%≤Si≤0.61%, 1.29%≤Mn≤1.6%, S≤0.0085%, P≤0.017, and the remainder is Fe.
[0033] Preferably, the flux-cored welding wire is prepared with TiO in a mass ratio of 36-40:3.5-5.5:1.0-1.6:0.98-2.94 2 、SiO 2 、Al 2 O 3 , NaF, during the U-rib upward internal welding process, the melting point is maintained in the range of 990-2050℃.
[0034] TiO 2 、SiO 2 、Al 2 O 3The components of NaF are mixed in the above-mentioned specific proportions. The resulting mixture can not only ensure that it has a high melting point and can support the molten liquid metal to prevent it from flowing downward, but also ensure that the weld seam inside the U rib is beautiful in shape. During the welding process, due to the action of the arc, this mixture can release more ionized substances to stabilize the arc and ensure the sufficient burning of the arc.
[0035] Furthermore, the flux-cored welding wire also contains magnesium powder, metallic manganese, and silicon-manganese alloy, and the mass ratio is 3-5:2-4:18-22, and the mass ratio of silicon to manganese in the silicon-manganese alloy is preferably 17:65. These components are sequentially desulfurized and deoxidized in the early, middle, and late stages of the U-rib internal welding process, and play a role at the melting point of each stage, completely removing the oxide inclusions in the weld, ensuring the purity of the weld metal, and at the same time, the alloy transition is sufficient, ensuring the high toughness of the weld metal.
[0036] When preparing the flux-cored welding wire for Q345qD steel of the present invention, the flux-cored material is preferably formulated according to the following components in mass percentage: 38-42% of rutile, 5-8% of feldspar, 1-3% of sodium fluoride, 18-22% of silicon-manganese alloy, 2-4% of metallic manganese, 3-6% of magnesium powder, and iron powder is supplemented to 100%. The flux-cored wire is wrapped with a welding wire sheath; the flux-cored material is filled in the welding wire sheath at a filling rate of 13.5-15.0%. The welding wire sheath is made of low-carbon steel material or low-alloy steel material; the diameter of the flux-cored welding wire is 1.2mm to 1.4mm.
[0037] The flux core material for welding wire provided by the present invention has the following functions for each component constituting the flux core welding wire for Q345qD steel:
[0038] Rutile: Its main function is to form slag and stabilize arc. The main component of rutile is TiO 2 , which can adjust the solidification speed of the slag, improve the droplet transition and enhance the arc stability.
[0039] Feldspar: The main function is to stabilize the arc. Feldspar contains high levels of KO and Na. 2 O, which has the function of stabilizing the welding arc and helps to stabilize the welding process. Because the high melting point components in feldspar may affect the viscosity and slag removal of the slag, the amount of feldspar added needs to be properly controlled to adjust the properties of the slag.
[0040] Sodium fluoride: Its main function is to improve the quality of welds and increase welding efficiency, because sodium fluoride can form an antioxidant protective layer during the welding process, effectively protect the weld area, reduce oxidation and the formation of impurities, and improve the uniformity and strength of the weld, thereby improving the quality of the weld; because sodium fluoride can improve the stability of the arc, promote the formation and continuation of the arc, and reduce the melting temperature, thereby increasing the welding speed and efficiency.
[0041] Silicon-manganese alloy: The main function of silicon (Si) is to refine carbide grains and improve the strength of the matrix. An appropriate amount of silicon content helps to improve welding quality, but too low a silicon content may lead to oxidation pores and burnout of alloy elements; manganese (Mn) is an important element for desulfurization and deoxidation. Its main function is to refine austenite grains, eliminate non-metallic inclusions, and improve the toughness of the cladding alloy.
[0042] Manganese metal: Its main function is to improve the hardness and toughness, and enhance the durability of welding wire; it can adjust the composition of the molten pool, making the welding process more stable. Manganese metal is used as a deoxidizer, and can also react with sulfur to form manganese sulfide, thereby reducing the tendency of thermal cracks in the weld caused by sulfur.
[0043] Magnesium powder: used as a reducing agent or additive to improve welding performance.
[0044] Iron powder: Its main function is to enhance the fluidity and permeability of welding materials, so that the molten metal flows into the welding joint faster and ensures the welding quality. Iron powder can also accelerate the reduction process of iron oxides and help remove oxides.
[0045] When Q345qD steel flux-cored welding wire made of the above-mentioned various components is used for welding, the weld is beautifully formed and slag is easy to remove; the weld joint has excellent mechanical properties and high toughness.
[0046] The following examples, unless otherwise stated, were prepared by the following method:
[0047] 1) Drying the components of the flux core material for welding wire for the first time, then adding them into a powder mixer and stirring and mixing them evenly, and then drying the evenly mixed flux core material for welding wire for the second time to obtain a dry powder mixture of the flux core material for welding wire;
[0048] 2) Roll the steel strip used as the outer skin of the welding wire into a U-shaped groove;
[0049] 3) Filling the dry powder mixture of the welding wire core material into the U-shaped groove;
[0050] 4) The U-shaped groove containing the dry powder mixture of the flux core material is closed and rolled into an O-shape, and then drawn to the set diameter of the welding wire.
[0051] It should be noted that, as a preferred embodiment of the flux-cored welding wire for Q345qD steel provided by the present invention, TiO 2 The content is more than 98%, and the impurity S and P content are very low; the feldspar is baked anhydrous feldspar; the mass ratio of silicon to manganese in the silicon-manganese alloy is 17:65, and the magnesium powder is atomized spheroidized. The use of Q345qD steel flux-cored welding wire that meets the requirements of the above components can ensure its welding process performance and mechanical properties.
[0052] Example 1
[0053] A flux core material for welding wire, comprising the following components in percentage by mass:
[0054] Rutile: 38%, feldspar: 5%, sodium fluoride 2%, silicon manganese alloy 20%, metallic manganese 3%, magnesium powder 4%, and the rest is iron powder added to 100%.
[0055] A flux-cored welding wire for Q345qD steel comprises the above-mentioned flux-cored material for the welding wire and a low-carbon steel strip as a welding wire outer sheath.
[0056] Example 2
[0057] A flux core material for welding wire, comprising the following components in percentage by mass:
[0058] Rutile: 40%, feldspar: 6%, sodium fluoride 1%, silicon manganese alloy 18%, metallic manganese 4%, magnesium powder 5%, and the rest is iron powder added to 100%.
[0059] A flux-cored welding wire for Q345qD steel comprises the above-mentioned flux-cored material for the welding wire and a low-carbon steel strip as a welding wire outer sheath.
[0060] Example 3
[0061] A flux core material for welding wire, comprising the following components in percentage by mass:
[0062] Rutile: 42%, feldspar: 8%, sodium fluoride 1%, silicon manganese alloy 22%, metallic manganese 2%, magnesium powder 3%, and the rest is iron powder added to 100%.
[0063] A flux-cored welding wire for Q345qD steel comprises the above-mentioned flux-cored material for the welding wire and a low-carbon steel strip as a welding wire outer sheath.
[0064] Example 4
[0065] A flux core material for welding wire, comprising the following components in percentage by mass:
[0066] Rutile: 39%, feldspar: 7%, sodium fluoride 3%, silicon manganese alloy 19%, metallic manganese 2%, magnesium powder 3%, and the rest is iron powder added to 100%.
[0067] A flux-cored welding wire for Q345qD steel comprises the above-mentioned flux-cored material for the welding wire and a low-carbon steel strip as a welding wire outer sheath.
[0068] Example 5
[0069] A flux core material for welding wire, comprising the following components in percentage by mass:
[0070] Rutile: 38%, feldspar: 5%, sodium fluoride 2%, silicon manganese alloy 18%, metallic manganese 3%, magnesium powder 6%, and the rest is iron powder added to 100%.
[0071] A flux-cored welding wire for Q345qD steel comprises the above-mentioned flux-cored material for the welding wire and a low-carbon steel strip as a welding wire outer sheath.
[0072] Example 6
[0073] A flux core material for welding wire, comprising the following components in percentage by mass:
[0074] Rutile: 39%, feldspar: 6%, sodium fluoride 3%, silicon manganese alloy 21%, metallic manganese 2%, magnesium powder 6%, and the rest is iron powder added to 100%.
[0075] A flux-cored welding wire for Q345qD steel comprises the above-mentioned flux-cored material for the welding wire and a low-carbon steel strip as a welding wire outer sheath.
[0076] Example 7
[0077] A flux core material for welding wire, comprising the following components in percentage by mass:
[0078] Rutile: 41%, feldspar: 7%, sodium fluoride 2%, silicon manganese alloy 21%, metallic manganese 4%, magnesium powder 4%, and the rest is iron powder added to 100%.
[0079] A flux-cored welding wire for Q345qD steel comprises the above-mentioned flux-cored material for the welding wire and a low-carbon steel strip as a welding wire outer sheath.
[0080] The Q345qD steel flux-cored welding wire based on Examples 1-7 was used for the U-rib upward internal welding of the Q345qD steel bridge, and the experimental results obtained are as follows:
[0081] Table 1 Comparison of experimental results of supine welding
[0082] Model No. Weld seam forming Appearance quality Existing welding wire Local sagging phenomenon, poor weld formation Slag inclusions are present locally Flux cored wire 1 Slight sagging phenomenon, good weld formation good Flux cored wire 2 Slight drop phenomenon, good weld formation good Flux cored wire 3 Slight drop phenomenon, good weld formation good Flux cored wire 4 Slight sagging phenomenon, good weld formation good Flux cored wire 5 Slight drop phenomenon, good weld formation good Flux cored wire 6 Slight sagging phenomenon, good weld formation good Flux cored wire 7 Slight sagging phenomenon, good weld formation good
[0083] By comparing the test results in the above table, it can be seen that the viscosity of the molten iron formed by the flux-cored welding wires 1-7 for Q345qD steel of the present invention increases to varying degrees, which can reduce the phenomenon of molten iron falling to varying degrees, and the shape and appearance of the weld are excellent, and there is no welding defect such as slag inclusion in the welded part, which effectively improves the forming quality of the supplementary inner weld. Among them, the flux-cored welding wire 1 has the outstanding advantages of high viscosity and high toughness, such as Figure 1 As shown, the appearance quality can be taken into consideration during the internal welding process in the upward position, and the internal welding effect in the upward position is the best. The main reason is that the flux-cored welding wire for Q345qD steel provided by the present invention contains TiO 2 Rutile, the main component of which is SiO 2 、Al2 O 3 The feldspar, sodium fluoride (NaF) and other ingredients are mixed in a specific proportion of the components of the present invention. The resulting mixture can not only ensure that it has a high melting point, can lift the molten liquid metal and prevent it from flowing downward, but also ensure that the weld is beautifully formed; during the welding process, due to the action of the arc, this mixture can release more ionized substances to stabilize the arc and ensure the sufficiency of the arc combustion; the Q345qD steel flux-cored welding wire provided by the present invention also contains magnesium powder, metal manganese, and silicon-manganese alloy combinations that can deoxidize, purify weld metal and transition alloys. Because the melting points of the above three material components are different, during the welding process, deoxidation is carried out in the early, middle and late stages in turn to completely remove the oxidized inclusions in the weld to ensure the purity of the weld metal. At the same time, the alloy transition is sufficient to ensure the high toughness of the weld metal.
[0084] Example 8
[0085] This embodiment provides the application of the Q345qD steel flux-cored welding wire prepared in the above-mentioned embodiments 1-7 in the U-rib upward internal welding of the Q345qD steel bridge. Simulating the working environment of the U-rib upward internal welding of the Q345qD steel bridge, the Q345qD steel flux-cored welding wire with a diameter of 1.2 mm and 1.4 mm prepared in the embodiments 1-7 is welded according to the following process parameters: the shielding gas is CO 2 , welding is carried out in overhead welding position, current 200-220A, voltage 22-24V, welding speed 24-27cm / min.
[0086] It should be noted that, in actual application, the flux-cored welding wire for Q345qD steel is used in the overhead internal welding process of the U-rib of Q345qD steel bridge. The flux-cored welding wire for Q345qD steel is carried by an overhead internal welding robot to enter the interior of the U-rib for welding; the welding current is: 200-220A, the welding voltage is 20-24V, and the welding speed is 0.25-0.30m / min for overhead welding of the interior of the U-rib.
[0087] It should be noted that, as a preferred embodiment, the chemical composition of the flux-cored welding wire for Q345qD steel provided by the present invention includes, by mass percentage: 0.035%≤C≤0.06%, 0.4%≤Si≤0.61%, 1.29%≤Mn≤1.6%, S≤0.0085%, P≤0.017, and the balance is Fe; the flux-cored welding wire for Q345qD steel contains TiO 2 、SiO 2 、Al 2 O 3 , NaF, and TiO 2 、SiO 2 、Al 2 O 3, NaF in a specific mass ratio of 36-40:3.5-5.5:1.0-1.6:0.98-2.94, and during the welding process, the melting point is maintained in the range of 990-2050°C; the Q345qD steel flux-cored welding wire also contains magnesium powder, metallic manganese, and silicon-manganese alloy, and the specific mass ratio of magnesium powder, metallic manganese, and silicon-manganese alloy is 3-5:2-4:18-22, and desulfurization and deoxidation reactions are carried out in the early, middle, and late stages of the welding process respectively; the mass ratio of silicon to manganese in the silicon-manganese alloy is 17:65.
[0088] Table 2 Mechanical properties of Q345qD steel flux-cored welding wire deposited metal of Examples 1-7
[0089]
[0090] Note: The specified value of impact energy for thin steel plate joints with thickness less than or equal to 20mm is 27J.
[0091] Table 3 Chemical composition of the deposited metal of the flux-cored wire for Q345qD steel of Examples 1-7 (wt%)
[0092]
[0093]
[0094] The foregoing description of specific exemplary embodiments of the present invention has been presented for the purpose of illustration and description. It is not intended to exclude or limit the present invention to the precise form disclosed, and it is obvious that many modifications and changes are feasible in view of the above teachings. Exemplary embodiments are selected and described to explain certain principles of the present invention and their practical application, so that other technicians in the field can make or use various exemplary embodiments of the present invention, and various alternatives and modifications thereof. It is intended that the scope of the present invention will be defined by the claims attached hereto and their equivalents.
[0095] It is to be understood that the above embodiments are merely exemplary embodiments adopted to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered as the protection scope of the present invention. In the description of this specification, the description of reference terms "an embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms need not be directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
Claims
1. Application of Q345qD steel flux-cored welding wire in U-rib upward internal welding of steel bridges, characterized in that: The chemical components in the flux-cored welding wire include, by mass percentage: 0.035%≤C≤0.06%, 0.4%≤Si≤0.61%, 1.29%≤Mn≤1.6%, S≤0.0085%, P≤0.017, and the balance is Fe.
2. The use according to claim 1, characterized in that: The flux-cored welding wire contains TiO2, SiO2, Al2O3, and NaF, and the specific mass ratio of TiO2, SiO2, Al2O3, and NaF is 36-40: 3.5-5.5:1.0-1.6:0.98-2.94, during the welding process, the melting point is maintained in the range of 990-2050℃.
3. The use according to claim 2, characterized in that: The flux-cored welding wire also contains magnesium powder, metallic manganese, and silicon-manganese alloy, and the specific mass ratio of magnesium powder, metallic manganese, and silicon-manganese alloy is 3-5:2-4:18-22, and desulfurization and deoxidation reactions are carried out in the early, middle, and late stages of the welding process respectively.
4. The use according to claim 3, characterized in that: The mass ratio of silicon to manganese in the silicon-manganese alloy is 17:
65.
5. The use according to claim 1, characterized in that: The flux-cored welding wire comprises a flux core material for the welding wire and a welding wire sheath.
6. The use according to claim 5, characterized in that: The welding wire flux core material is filled in the welding wire sheath at a filling rate of 13.5-15.0%.
7. The use according to claim 5 or 6, wherein the flux core material for welding wire comprises the following components in percentage by mass: 38-42% rutile, 5-8% feldspar, 1-3% sodium fluoride, 18-22% silicon manganese alloy, 2-4% metallic manganese, 3-6% magnesium powder, and iron powder is supplemented to 100%.
8. The use according to claim 7, characterized in that: The welding wire outer sheath is made of low carbon steel material or low alloy steel material.
9. The use according to claim 7, characterized in that: The diameter of the flux-cored welding wire is 1.2 mm to 1.4 mm.
10. The use according to claim 5, characterized in that: The preparation method of the flux-cored welding wire comprises the following steps: 1) Drying the components of the flux core material for welding wire for the first time, adding them into a powder mixer and stirring and mixing them evenly, and then drying the evenly mixed flux core material for welding wire for the second time to obtain a dry powder mixture of the flux core material for welding wire; 2) Roll the steel strip used as the outer skin of the welding wire into a U-shaped groove; 3) Filling the dry powder mixture of the welding wire core material into the U-shaped groove; 4) The U-shaped groove containing the dry powder mixture of the flux core material is closed and rolled into an O-shape, and then drawn to the set diameter of the welding wire.
Citation Information
Patent Citations
Gas-shielded flux-cored wire for maritime engineering
CN103692110A
High-strength and high-toughness gas shielded flux-cored wire used for bridge steel
CN106334884A
Ultra-low hydrogen type acid flux-cored wire and production method thereof
CN111702371A
Upward welding installation method of seismic mitigation and isolation support for steel bridge
CN116000416A
Flux cored wire for welding stainless steel
JP1997201696A