Stirring device and method for preparing low Mooney white carbon black / natural latex composite material by adopting same
Through homemade spherical ribbon stirring device and high-temperature flash evaporation device, combined with emulsifier and silane coupling agent, the problems of uneven stirring and Mooneygo in the wet mixing process are solved, and white carbon black/natural latex composite is achieved The uniform dispersion of the materials and the low Mooney characteristics improve the processing performance and production efficiency of the glue.
Patent Information
- Application Number
- CN202411169470.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-24
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing wet mixing process, the mixing and dispersion are uneven, the filler is dispersed unevenly, the use of flocculants affects the performance of the glue, increases environmental pollution and wastewater treatment costs, and the Mooney is a high wet mixing rubber, which increases rubber. Difficulty in subsequent processing.
The homemade spherical ribbon stirring device is used for uniform stirring without dead angles, combining emulsifier and silane coupling agent to promote the dispersion of white carbon black, and rapid dehydration and drying is achieved through high-temperature flash evaporation device, using a two-step kneading process and modification additives Improve master glue performance.
The uniform dispersion of white carbon black/natural latex composite materials is achieved, which reduces Mooney, improves the processing performance and production efficiency of the rubber, reduces environmental pollution, and significantly improves the physical and dynamic mechanical properties.
Smart Images

Figure CN118977333A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of natural rubber wet mixing, and in particular relates to a stirring device and a method for preparing a low Mooney white carbon black / natural latex composite material by using the stirring device. Background Art
[0002] Carbon black is the most widely used and largest amount of reinforcing filler in rubber / composite materials. The addition of carbon black gives rubber excellent comprehensive physical and mechanical properties. However, due to excessive energy consumption and outdated process technology causing serious pollution to the global environment, the tire industry urgently needs to reduce energy consumption and environmental pollution, and improve tire performance and technological content. In 1992, Michelin Green Tire successfully added silica (i.e. white carbon black) as a carbon black substitute to tire tread rubber, reducing rolling resistance and improving wet skid resistance without affecting tire grip and wear resistance.
[0003] Although the traditional dry mixing process can improve the mixing quality, the mixing consumes a lot of energy, the processing process is dusty, the working environment is poor, it harms the health of the workers, and the quality stability of the product is poor. Wet mixing technology is a mixing process applied to the preparation of composite materials from rubber in an emulsion state. The latex and reinforcing materials are mixed under liquid phase conditions. Compared with the dry mixing process, the entire wet mixing process is efficient and dust-free. Chinese invention patent CN102153792 discloses a method for preparing natural rubber materials by wet mixing, which adopts a method of preparing natural rubber masterbatch by adding acetic acid to the mixed liquid for flocculation. The processing technology is simple and the dust pollution in the production process is small. Furthermore, in a method for preparing white carbon black NR / masterbatch for tire belt layer disclosed in Chinese invention patent CN104311906, the white carbon black / NR masterbatch is prepared by high-speed stirring and acid coagulation, which effectively shortens the time for mixing a large amount of white carbon black, reduces energy consumption, and expands the number of fillers in rubber. Chinese invention patent CN110802758 discloses a gas-assisted spraying rubber wet mix production equipment and production method, which is used to solve the current problems of wet mix production process and production equipment being numerous and unevenly dispersed.
[0004] However, in the above existing patent technologies, stirring and dispersing cannot achieve uniform stirring without dead angles, resulting in uneven dispersion of fillers. Moreover, although acid can be used as a flocculant for rapid flocculation, the gelling material by adding acid or salt has a great influence on the performance of the rubber material, and the performance of the produced mixed rubber is unstable, which also increases the potential possibility of environmental pollution and the cost of wastewater treatment. In addition, since a large amount of white carbon black is filled in natural rubber during wet mixing, the Mooney viscosity of the wet mixed rubber is relatively high, which increases the difficulty of subsequent processing of the rubber. Summary of the invention
[0005] The purpose of the present invention is to solve the above problems existing in the prior art, and proposes a stirring device and a method for preparing a low Mooney white carbon black / natural latex composite material using the same. The present invention adopts a wet mixing masterbatch preparation process, and realizes uniform dispersion without dead angles through a stirring device independently developed, thereby overcoming the shortcomings of the prior art such as the use of flocculants and long processing time. At the same time, two-step mixing is used to further improve the good dispersion of fillers, and the problem of large Mooney and difficult processing of the masterbatch is improved with the help of modified additives, so as to realize the green preparation of rubber composite materials and obtain a white carbon black / natural latex composite material with low Mooney.
[0006] The technical solution of the present invention is:
[0007] The present invention provides a stirring device, comprising a device body and a support, the device body comprising a stirring tank and a first motor for driving the stirring tank to rotate, the outside of the stirring tank is sequentially sleeved with an internal support rotating frame and an external support rotating frame, the internal support rotating frame is connected to the stirring tank through a rotating shaft; the stirring tank is spherical, and a screw-belt stirring paddle and a main blade are longitudinally arranged inside the stirring tank, the main blade is spiral, the screw-belt stirring paddle surrounds the main blade and is spherical; the stirring tank is also equipped with a second motor for driving the screw-belt stirring paddle and the main blade to rotate.
[0008] Furthermore, a feed port is provided at the upper end of the tank body of the stirring tank, and a discharge port is provided at the lower end, the two ends of the main blade are respectively connected to the upper end and the lower end of the tank body, and the two ends of the spiral belt stirring paddle are respectively connected to the upper end and the lower end of the tank body.
[0009] Furthermore, the stirring tank is connected to the first motor via a rotating connecting block, and the stirring tank rotates when driven by the first motor.
[0010] Furthermore, it also includes a support for supporting the main body of the device, the support includes a base and brackets vertically arranged at both ends of the base, the external support rotating frame is connected to the brackets on both sides through a rotating shaft, and the internal support rotating frame is connected to the external support rotating frame through a rotating shaft.
[0011] The present invention also provides a method for preparing a low Mooney silica / natural rubber latex composite material using any one of the stirring devices described above, comprising the following steps:
[0012] (1) weighing a silane coupling agent, an emulsifier and a rubber lubricant according to a formula, emulsifying and homogenizing for 10 to 20 minutes to obtain an additive dispersion, injecting the additive dispersion and the white carbon black slurry into a stirring device in sequence for stirring and mixing, adjusting the speed of the ribbon stirring paddle and the main paddle in the stirring tank to 5000 to 30000 r / min, the speed of the stirring tank to 10 to 300 r / min, and the stirring time to 5 to 10 minutes to prepare a first mixed solution that is mixed evenly;
[0013] (2) weighing natural rubber latex according to the formula and adding it into a stirring tank, and fully stirring and mixing it with the first mixed liquid, the speed of the ribbon stirring paddle and the main paddle in the stirring tank is set to 5000-30000 r / min, the speed of the stirring tank is 10-300 r / min, and the stirring time is 5-10 min to obtain a second mixed liquid;
[0014] (3) placing the second mixed solution at 135-145° C. for flocculation, rapid dehydration and drying, and then pressing it into thin sheets, and drying it in an oven at 60-100° C. until the water content of the rubber material drops below 1%, thereby obtaining a modified silica / natural rubber latex masterbatch;
[0015] (4) Mixing the silica / natural rubber latex masterbatch with zinc oxide and stearic acid in the formula in an internal mixer for 5 to 6 minutes to obtain a rubber compound, and then mixing the rubber compound with sulfur and NS in an open mixer to obtain a silica / natural rubber latex composite material.
[0016] Further, the formula includes 100phr of natural latex, 30-40phr of white carbon black, 3-5phr of silane coupling agent, 2-4phr of emulsifier, 1-3phr of rubber lubricant, 4-6phr of zinc oxide, 1-3phr of SAD, 1-3phr of sulfur, and 1-2phr of NS;
[0017] The natural latex is one or more of fresh latex, concentrated latex, concentrated natural latex or concentrated natural skim latex.
[0018] Further, the silane coupling agent is selected from one or more of γ-aminopropyltriethoxysilane (KH550), γ-glycidoxypropyltrimethoxysilane (KH560), γ-(methacryloyloxy)propyltrimethoxysilane (KH570), γ-mercaptopropyltrimethoxysilane (KH590), bis-(γ-triethoxysilylpropyl)-tetrasulfide (Si69), bis-(γ-triethoxysilylpropyl)-disulfide (Si75), and γ-mercaptopropyl-ethoxybis(propyl-hexapropoxy)siloxane (Si747);
[0019] The emulsifier is selected from one or more of sodium dodecyl sulfate (SDS), dodecylphenol polyoxyethylene ether (OP-10), nonylphenol polyoxyethylene ether (TX-10), polyethylene glycol (PEG), stearic acid monoethanolamide (SMEA), and fatty alcohol polyoxyethylene ether (AEO-9);
[0020] The rubber lubricant is selected from one or more of talcum powder, mica powder, calcium carbonate, clay, and calcium terephthalate.
[0021] Furthermore, in step (3), the second mixed liquid is placed on a high-temperature flash evaporation device for flocculation and rapid dehydration and drying, wherein the high-temperature flash evaporation device comprises a high-temperature flash evaporation roller, wherein the high-temperature flash evaporation roller has a cylindrical shell structure and an inner cavity, wherein the inner cavity stores heat transfer oil to ensure uniform heating of the surface of the high-temperature flash evaporation roller;
[0022] The high-temperature flash evaporation device also includes a baffle groove, a mold temperature controller for providing heating, and a third motor for driving the high-temperature flash evaporation round roller to roll at a uniform speed. The rotation speed of the high-temperature flash evaporation round roller is 10-100r / min, and its surface temperature is 135-145°C.
[0023] Furthermore, when the second mixed liquid is transported to the surface of the high-temperature flash roller at a temperature of 135-145°C through the baffle groove, its water evaporates rapidly to form a molded rubber compound that adheres to the surface of the high-temperature flash roller and rolls with the high-temperature flash roller. When it rolls 5-8 times and the surface of the rubber compound is tight and has no obvious sticky lumps, the drying is completed, and the dried mother film is scraped off to complete the flocculation and dehydration cycle.
[0024] Furthermore, in the step (1), the rotation speed of the screw-ribbon agitator and the main blade is 10000 r / min, and the rotation speed of the stirring tank is 100 r / min; in the step (2), the rotation speed of the screw-ribbon agitator and the main blade is set to 20000 r / min, and the rotation speed of the stirring tank is 200 r / min.
[0025] Beneficial effects of the present invention:
[0026] (1) Compared with the prior art, the present invention firstly adds mixed auxiliary ingredients including silane coupling agent, emulsifier and rubber lubricant by liquid phase method to promote chemical grafting and microscopic dispersion of white carbon black in rubber matrix; increases the surface grafting rate of white carbon black by emulsification with emulsifier, promotes the combination of silane coupling agent and white carbon black, reduces the silicon hydroxyl group on the surface of white carbon black, and thus reduces the adsorption of white carbon black on the promoter; rubber lubricant can reduce the friction resistance inside the rubber, reduce viscosity, improve storage stability, and improve processing performance, which helps to promote the dispersion of rubber and achieve better processing performance. Compared with the traditional dry mixing, the addition of multiple auxiliary agents reduces the polar groups on the surface of white carbon black, promotes the dispersion of white carbon black in the rubber matrix, and significantly improves the mechanical properties.
[0027] (2) The present invention realizes uniform stirring and mixing without dead angles by means of the rotation of the spherical spiral-ribbon stirring blade inside the self-made stirring device and the external stirring tank. The internal stirring blade and the stirring tank body have different directions and rotation speeds, thereby realizing uniform preparation of the mixed liquid; then the mixed liquid is poured onto a high-temperature flash evaporation roller for rapid dehydration and drying. With the help of the high-temperature flash evaporation roller, dehydration and drying can be carried out efficiently and continuously, and then mixing is performed to obtain a silica / natural latex composite material. High-speed stirring and high-temperature flash evaporation processes improve work efficiency, and silica achieves a microscopic dispersion effect in the rubber matrix, which can further prepare a mixed rubber with uniform quality.
[0028] (3) The method of the present invention is used to prepare the rubber compound. Not only are the physical properties and dynamic mechanical properties significantly improved compared to the rubber compound prepared by the traditional mixing process, but the production cycle is also shortened, the problem of flying white carbon black and rubber additives is avoided, and the rubber production efficiency is improved. The masterbatch prepared by the wet process also has a lower Mooney value and better processing performance.
[0029] (4) The self-made stirring device provided by the present invention can realize the uniform dispersion of white carbon black particles in latex, and the high-temperature flash evaporation device provided improves the flocculation and drying efficiency. In addition, the preparation method of the present invention does not require the addition of acids and other flocculants, does not corrode equipment, does not generate irritating odor, reduces environmental pollution, and has good stability, shortened production cycle, low Mooney, and good processing performance, thereby realizing continuous industrial production of high-quality rubber. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a structural diagram of the stirring device provided by the present invention;
[0031] Figure 2 It is a structural diagram of the external rotating part of the stirring device;
[0032] Figure 3 It is the internal structure diagram of the stirring tank in the stirring device;
[0033] Figure 4 is an axonometric diagram of the high-temperature flash evaporation device provided by the present invention;
[0034] Figure 5 It is a structural diagram of the high-temperature flash evaporation device provided by the present invention;
[0035] In the above figures, 1. first motor; 2. device body; 3. rotating connection block; 4. second motor; 5. stirring tank; 6. internal support rotating frame; 7. external support rotating frame; 8. feed inlet; 9. screw-ribbon stirring paddle; 10. main paddle; 11. discharge port; 12. mold temperature controller; 13. high-temperature flash steaming roller; 14. baffle groove; 15. main frame; 16. third motor; 17. scraper. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] In order to further understand the present invention, the present invention will be further described in conjunction with the accompanying drawings and embodiments.
[0038] Example 1
[0039] like Figure 1 As shown, this embodiment provides a stirring device, including a device body 2 and a support, wherein the device body 2 includes a first motor 1, a rotating connection block 3, a stirring tank 5, a second motor 4, an internal support rotating frame 6 and an external support rotating frame 7. The output shaft of the first motor 1 is connected to the stirring tank 5 through the rotating connection block 3 and is used to drive the stirring tank 5 to rotate, and the first motor 1 and the second motor 4 are both connected to a power source to provide power.
[0040] like Figure 2 As shown, both the internal support rotating frame 6 and the external support rotating frame 7 are square frame structures, and the external support rotating frame 7 is sleeved outside the internal support rotating frame 6, and the two are connected by a rotating shaft. The stirring tank 5 is spherical, and the spherical stirring tank 5 is arranged in the middle of the internal support rotating frame 6, and is also rotatably connected to the internal support rotating frame 6 through the rotating shaft. That is, the internal support rotating frame 6 is connected to the stirring tank 5 inside, and is connected to the external support rotating frame 7 outside.
[0041] Furthermore, the stirring device also includes a support for supporting the device body 2, the support includes a base and brackets vertically arranged at both ends of the base, an external support rotating frame 7 is installed between the two brackets, and the external support rotating frame 7 is connected to the brackets on both sides through a rotating shaft.
[0042] like Figure 3 As shown, a ribbon stirring paddle 9 and a main blade 10 are arranged inside the stirring tank 5. The ribbon stirring paddle 9 and the main blade 10 are both longitudinally installed in the stirring tank 5, and the ribbon stirring paddle 9 is arranged around the main blade 10. The two ends of the main blade 10 are respectively connected to the upper end and the lower end of the stirring tank 5. Similarly, the two ends of the ribbon stirring paddle 9 are respectively connected to the upper and lower ends of the stirring tank 5. A second motor 4 is installed at the upper end of the stirring tank 5. The output shaft of the second motor 4 is connected to the upper ends of the ribbon stirring paddle 9 and the main blade 10, and drives the ribbon stirring paddle 9 and the main blade 10 to rotate in the stirring tank 5.
[0043] It should be noted that the stirring tank 5 is spherical, which can achieve uniform stirring without dead angles. The main blade 10 is spiral and installed in the middle of the spherical stirring tank 5. The screw-ribbon stirring paddle 9 surrounds the main blade 10 and is spherical. The outer diameter of the spherical screw-ribbon stirring paddle 9 is slightly smaller than the inner diameter of the stirring tank 5, so that the materials in the stirring tank 5 can be fully and completely stirred and mixed. The screw-ribbon stirring paddle 9 and the main blade 10 rotate at a high speed under the drive of the second motor 4, cooperate with each other, and improve the mixing efficiency; at the same time, the stirring tank 5 is also driven by the first motor 1 to swing, thereby improving the turbulent effect inside the stirring tank 5.
[0044] Furthermore, the upper end of the tank body of the stirring tank 5 is provided with a feed port 8 for adding materials, and the lower end is provided with a discharge port 11 for discharging materials.
[0045] Example 2
[0046] like Figure 4 and Figure 5 As shown, this embodiment provides a high-temperature flash evaporation device for flocculating and rapidly dehydrating the second mixed liquid, wherein the main structure is a high-temperature flash evaporation roller 13 of a cylindrical shell structure, and the inner cavity of the high-temperature flash evaporation roller 13 stores heat transfer oil to ensure uniform heating of the surface of the high-temperature flash evaporation roller 13. The device also includes a main frame 15 for mounting the high-temperature flash evaporation roller 13 and supporting it.
[0047] The mold temperature controller 12 provides heating, and the heat transfer oil in the oil storage tank is transported to the cavity of the high-temperature flash round roller 13 through the mold temperature controller circulation pump, thereby ensuring uniform heating of the surface of the high-temperature flash round roller 13, and its surface temperature can reach 135-145° C. The high-temperature flash device also includes a third motor 16 for driving the high-temperature flash round roller 13 to roll at a uniform speed.
[0048] The high-temperature flash evaporation device is provided with a baffle groove 14 at the upper part and a scraper 17 at the lower part. When working, the high-temperature flash evaporation roller 13 rolls at a uniform speed of 10-100r / min; the mixed liquid is introduced from the upper baffle groove 14, and after contacting the high-temperature flash evaporation roller 13 with a temperature of 135-145°C, the water evaporates rapidly, and the molded rubber adheres to the surface of the high-temperature flash evaporation roller 13 and rolls with the high-temperature flash evaporation roller 13; when the high-temperature flash evaporation roller 13 rotates 5-8 times, the surface of the rubber is tight and there is no obvious sticky block, and it is considered that the drying is completed; the scraper 17 is close to the surface of the high-temperature flash evaporation roller 13, and the dried mother film is scraped off, and the flocculation and dehydration steps are completed in a cycle.
[0049] Example 3
[0050] This embodiment provides a method for preparing a low Mooney silica / natural rubber latex composite material using the above-mentioned stirring device and high-temperature flash evaporation device, comprising the following steps:
[0051] (1) Preparation of the first mixed solution
[0052] Weigh 2g of fatty alcohol polyoxyethylene ether, 3g of silane coupling agent Si69, 1.75g of calcium terephthalate, and 128.25g of deionized water, mix them, and place them in an ultrasonic disperser for 15min to obtain an additive dispersion, then add the additive dispersion and 140g of white carbon black slurry (solid content 25%) from the feed port into a stirring device for stirring and mixing, adjust the speed of the spiral ribbon stirring paddle and the main blade in the stirring tank to 10000r / min, the speed of the stirring tank body to 100r / min, the stirring time to 10min, rely on the rotation of the spiral ribbon stirring paddle, the main blade and the stirring tank to stir and disperse the mixed additive dispersion and the white carbon black slurry to prepare a first mixed solution that is evenly mixed;
[0053] (2) Preparation of the second mixed solution
[0054] Weigh 167 g of 60 wt% natural latex NRL into a stirring tank, stir and mix it with the first mixed solution, adjust the speed of the stirring paddle in the stirring tank to 20000 r / min, the speed of the stirring tank body to 200 r / min, and the stirring time to 10 min to obtain a second mixed solution;
[0055] (3) Flocculation and dehydration
[0056] The second mixed liquid is poured onto a high-temperature flash round roller at 145°C to rapidly dehydrate the second mixed liquid and dry it into a thin sheet, which is then placed in an oven at 90°C for subsequent drying. When the water content of the rubber material drops below 1%, it is taken out to obtain a modified silica / natural rubber latex masterbatch.
[0057] (4) Mixing
[0058] Put the white carbon black / natural rubber latex masterbatch, 5g zinc oxide and 2g stearic acid into an internal mixer and mix for 5 minutes to obtain a rubber mixture; then add 2.25g sulfur and 0.7g NS into the rubber mixture on an open mixer, and roll and triangle pack are alternately performed three times before unrolling.
[0059] The vulcanization characteristics of the rubber compound were measured by a rotorless vulcanizer. The vulcanization temperature was set to 150°C, the vulcanization pressure was set to 11 MPa, and the vulcanization time was set to T90×1.3. The mixed rubber was vulcanized to obtain a silica / natural rubber latex composite material.
[0060] Comparative Example 1
[0061] The natural rubber was selected as STR20 (Thailand No. 20 standard rubber), and STR20 was used to prepare the natural rubber composite material according to the following process, and the performance test was carried out:
[0062] According to the formula, 100g natural rubber STR20, 35g white carbon black, 3g silane coupling agent Si69, 5g zinc oxide, and 2g stearic acid were weighed. First, natural rubber was added to the internal mixer, and white carbon black, silane coupling agent Si69, zinc oxide, and stearic acid were added after 1 minute and 30 seconds. The mixing time was 5 minutes and 30 seconds, and the rubber discharge temperature was 145°C. The mixed rubber was discharged; then 2.25g sulfur and 0.7g accelerator NS were added to the open mixer. After the feeding was completed, the roll and triangle rubber were alternately rolled three times before the sheet was removed.
[0063] The vulcanization characteristics of the rubber compound were measured by a rotorless vulcanizer. The vulcanization temperature was set to 150°C, the vulcanization pressure was set to 11 MPa, and the vulcanization time was set to T90×1.3, and the mixed rubber was vulcanized and formed.
[0064] Comparative Example 2
[0065] This embodiment provides a method for preparing a low Mooney silica / natural rubber latex composite material using the above-mentioned stirring device and high-temperature flash evaporation device, comprising the following steps:
[0066] (1) Preparation of mixed solution
[0067] Weigh 140 g of white carbon black slurry (solid content 25%) and 167 g of 60 wt% natural latex NRL into a stirring tank, adjust the speed of the stirring paddle in the stirring tank to 10000 r / min, the speed of the stirring tank body to 100 r / min, and the stirring time to 10 min to obtain a first mixed solution;
[0068] (3) Flocculation and dehydration
[0069] The mixed liquid is poured onto a high-temperature flash round roller at 135°C to rapidly dehydrate the mixed liquid and dry into a thin sheet, and then placed in an oven at 60°C for subsequent drying. When the moisture content of the rubber material drops below 1%, it is taken out to obtain a modified silica / natural rubber latex masterbatch.
[0070] (4) Mixing
[0071] Put the white carbon black / natural rubber latex masterbatch, 3g of silane coupling agent Si69, 5g of zinc oxide and 2g of stearic acid into an internal mixer and mix for 5 minutes to obtain a rubber mixture; then add 2.25g of sulfur and 0.7g of NS into the rubber mixture on an open mixer, and roll and triangle pack alternately for three times before unrolling.
[0072] The vulcanization characteristics of the rubber compound were measured by a rotorless vulcanizer. The vulcanization temperature was set to 150°C, the vulcanization pressure was set to 11 MPa, and the vulcanization time was set to T90×1.3. The mixed rubber was vulcanized to obtain a silica / natural rubber latex composite material.
[0073] Example 4
[0074] This embodiment provides a method for preparing a low Mooney silica / natural rubber latex composite material using the above-mentioned stirring device and high-temperature flash evaporation device, comprising the following steps:
[0075] (1) Preparation of the first mixed solution
[0076] Weigh 3g of dodecylphenol polyoxyethylene ether, 4g of silane coupling agent KH550, 2g of calcium carbonate, and 126g of deionized water, mix them, and place them in an ultrasonic disperser for 10 minutes to obtain an additive dispersion liquid, then add the additive dispersion liquid and 140g of white carbon black slurry (solid content 25%) from the feed port into a stirring device for stirring and mixing, adjust the speed of the spiral ribbon stirring paddle and the main blade in the stirring tank to 5000r / min, the speed of the stirring tank body to 50r / min, and the stirring time to 10min, rely on the rotation of the spiral ribbon stirring paddle, the main blade and the stirring tank to stir and disperse the mixed additive dispersion liquid and the white carbon black slurry to prepare a first mixed liquid that is evenly mixed;
[0077] (2) Preparation of the second mixed solution
[0078] Weigh 167 g of 60 wt% natural latex NRL into a stirring tank, stir and mix it with the first mixed solution, adjust the speed of the stirring paddle in the stirring tank to 10000 r / min, the speed of the stirring tank body to 100 r / min, and the stirring time to 10 min to obtain a second mixed solution;
[0079] (3) Flocculation and dehydration
[0080] The second mixed liquid is poured onto a high-temperature flash round roller at 135°C to rapidly dehydrate the second mixed liquid and dry it into a thin sheet, which is then placed in an oven at 60°C for subsequent drying. When the water content of the rubber material drops below 1%, it is taken out to obtain a modified silica / natural rubber latex masterbatch.
[0081] (4) Mixing
[0082] Put the white carbon black / natural rubber latex masterbatch, 5g zinc oxide and 2g stearic acid into an internal mixer and mix for 5 minutes to obtain a rubber mixture; then add 2.25g sulfur and 0.7g NS into the rubber mixture on an open mixer, and roll and triangle pack are alternately performed three times before unrolling.
[0083] The vulcanization characteristics of the rubber compound were measured by a rotorless vulcanizer. The vulcanization temperature was set to 150°C, the vulcanization pressure was set to 11 MPa, and the vulcanization time was set to T90×1.3. The mixed rubber was vulcanized to obtain a silica / natural rubber latex composite material.
[0084] Example 5
[0085] This embodiment provides a method for preparing a low Mooney silica / natural rubber latex composite material using the above-mentioned stirring device and high-temperature flash evaporation device, comprising the following steps:
[0086] (1) Preparation of the first mixed solution
[0087] Weigh 4 g of stearic acid monoethanolamide, 5 g of silane coupling agent Si747, 1 g of mica powder, and 125 g of deionized water, mix them, and place them in an ultrasonic disperser for 20 min to obtain an additive dispersion, then add the additive dispersion and 140 g of white carbon black slurry (solid content 25%) from the feed port into a stirring device for stirring and mixing, adjust the speed of the ribbon stirring paddle and the main blade in the stirring tank to 20000 r / min, the speed of the stirring tank body to 200 r / min, the stirring time to 10 min, and stir and disperse the mixed additive dispersion and white carbon black slurry by rotating the ribbon stirring paddle, the main blade and the stirring tank to prepare a first mixed solution that is evenly mixed;
[0088] (2) Preparation of the second mixed solution
[0089] Weigh 167 g of 60 wt% natural latex NRL into a stirring tank, stir and mix it with the first mixed solution, adjust the speed of the stirring paddle in the stirring tank to 30000 r / min, the speed of the stirring tank body to 300 r / min, and the stirring time to 10 min to obtain a second mixed solution;
[0090] (3) Flocculation and dehydration
[0091] The second mixed liquid is poured onto a high-temperature flash round roller at 140°C to rapidly dehydrate the second mixed liquid and dry it into a thin sheet, which is then placed in an oven at 100°C for subsequent drying. When the water content of the rubber material drops below 1%, it is taken out to obtain a modified silica / natural rubber latex masterbatch.
[0092] (4) Mixing
[0093] Put the white carbon black / natural rubber latex masterbatch, 5g zinc oxide and 2g stearic acid into an internal mixer and mix for 6 minutes to obtain a rubber mixture; then add 2.25g sulfur and 0.7g NS into the rubber mixture on an open mixer, and roll and triangle pack are alternately performed three times before unrolling.
[0094] The vulcanization characteristics of the rubber compound were measured by a rotorless vulcanizer. The vulcanization temperature was set to 150°C, the vulcanization pressure was set to 11 MPa, and the vulcanization time was set to T90×1.3. The mixed rubber was vulcanized to obtain a silica / natural rubber latex composite material.
[0095] Test Example 1
[0096] The wet masterbatch prepared in Example 3, Example 4 and Comparative Example 1 was subjected to Mooney test, and the results are shown in Table 1.
[0097] Table 1 Wet masterbatch Mooney test results
[0098] Masterbatch Type ML(3+4)150℃ Comparative Example 2 142.13 Example 3 117.09 Example 4 121.90
[0099] The mechanical properties of the vulcanized rubber materials in Example 3, Example 4 and Comparative Example 1 were tested, and the results are shown in Table 2.
[0100] Table 2 Mechanical properties test results
[0101]
[0102]
[0103] Table 1 is a comparison of the Mooney values of the conventional wet masterbatch (Comparative Example 2) and the low Mooney masterbatch (Examples 3 and 4) prepared by the present invention. The emulsifier can increase the chemical grafting efficiency on the surface of silica through hydrogen bond physical adsorption and terminal hydroxyl chemical grafting, promote the combination of silane coupling agent and silica, and weaken the attraction between silica, which can effectively reduce the aggregation of silica and improve dispersion. The emulsifier promotes the combination of silane coupling agent and silica, and also reduces the silicon hydroxyl groups on the surface of silica, reducing the adsorption of silica to other promoters. The silane coupling agent enhances the interaction between rubber and filler, so that the dispersion and lubrication effect of the rubber lubricant are further exerted.
[0104] At the same time, with the help of a homemade stirring device, a spherical spiral-ribbon stirring paddle is used for stirring without dead angles, and the internal stirring blades and the stirring tank body have different directions and rotation speeds, so that the mixed liquid is evenly prepared. The prepared mixed liquid is poured onto a high-temperature flash round roller, and with the help of the high-temperature round roller, it can be efficiently and continuously dehydrated and dried. Since this process does not go through traditional raw rubber preparation processes such as acid flocculation and creping, the oxidation breakage or shear chain of the natural rubber molecular chain is reduced, so the rubber molecular chain is kept intact, and the Mooney of the low Mooney white carbon black / natural rubber masterbatch prepared by high-temperature flash evaporation in the present invention is reduced by 17% compared to the unmodified masterbatch, and has good processability of the rubber compound.
[0105] Table 2 is a comparison of mechanical properties of conventional rubber mix (Comparative Example 1), conventional wet-process rubber mix (Comparative Example 2) and modified silica / natural rubber latex mix prepared by the wet process of the present invention (Examples 3 and 4). The tensile and tearing mechanical properties of the wet-process rubber mix are better than those of the conventional dry-process mix, and the wet process greatly improves the dispersion of silica in the rubber matrix. T90 is the positive vulcanization time of the rubber compound, and the modified silica / natural rubber mix prepared by high-temperature flash evaporation increases the vulcanization rate and reduces energy consumption. Overall, the mechanical properties of the wet-process rubber mix prepared by the present invention are better than those of the conventional rubber mix.
[0106] The above description is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, modification, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A stirring device, It is characterized in that The invention comprises a device body and a support, wherein the device body comprises a stirring tank and a first motor for driving the stirring tank to rotate, an internal supporting rotating frame and an external supporting rotating frame are sequentially sleeved on the outside of the stirring tank, and the internal supporting rotating frame is connected to the stirring tank through a rotating shaft; the stirring tank is spherical, and a spiral-belt stirring paddle and a main blade are longitudinally arranged inside the stirring tank, the main blade is spiral, and the spiral-belt stirring paddle surrounds the main blade and is spherical; a second motor for driving the spiral-belt stirring paddle and the main blade to rotate is also installed on the stirring tank.
2. The stirring device according to claim 1, It is characterized in that The upper end of the tank body of the stirring tank is provided with a feed inlet, and the lower end is provided with a discharge port. The two ends of the main blade are respectively connected to the upper end and the lower end of the tank body, and the two ends of the spiral belt stirring paddle are respectively connected to the upper end and the lower end of the tank body.
3. The stirring device according to claim 1, It is characterized in that The stirring tank is connected to the first motor via a rotating connecting block, and the stirring tank rotates under the drive of the first motor.
4. The stirring device according to claim 1, It is characterized in that It also includes a support for supporting the device body, the support includes a base and brackets vertically arranged at both ends of the base, the external support rotating frame is connected to the brackets on both sides through a rotating shaft, and the internal support rotating frame is connected to the external support rotating frame through a rotating shaft.
5. A method for preparing a low Mooney silica / natural rubber latex composite material using the stirring device according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) weighing a silane coupling agent, an emulsifier and a rubber lubricant according to a formula, emulsifying and homogenizing for 10 to 20 minutes to obtain an additive dispersion, injecting the additive dispersion and the white carbon black slurry into a stirring device in sequence for stirring and mixing, adjusting the speed of the ribbon stirring paddle and the main paddle in the stirring tank to 5000 to 30000 r / min, the speed of the stirring tank to 10 to 300 r / min, and the stirring time to 5 to 10 minutes to prepare a first mixed solution that is mixed evenly; (2) weighing natural rubber latex according to the formula and adding it into a stirring tank, and fully stirring and mixing it with the first mixed liquid, the speed of the ribbon stirring paddle and the main paddle in the stirring tank is set to 5000-30000 r / min, the speed of the stirring tank is 10-300 r / min, and the stirring time is 5-10 min to obtain a second mixed liquid; (3) placing the second mixed solution at 135-145° C. for flocculation, rapid dehydration and drying, and then pressing it into thin sheets, and drying it in an oven at 60-100° C. until the water content of the rubber material drops below 1%, thereby obtaining a modified silica / natural rubber latex masterbatch; (4) Mixing the silica / natural rubber latex masterbatch with zinc oxide and stearic acid in the formula in an internal mixer for 5 to 6 minutes to obtain a rubber compound, and then mixing the rubber compound with sulfur and NS in an open mixer to obtain a silica / natural rubber latex composite material.
6. The method according to claim 5, It is characterized in that The formula includes 100phr of natural latex, 30-40phr of white carbon black, 3-5phr of silane coupling agent, 2-4phr of emulsifier, 1-3phr of rubber lubricant, 4-6phr of zinc oxide, 1-3phr of SAD, 1-3phr of sulfur, and 1-2phr of NS; The natural latex is one or more of fresh latex, concentrated latex, concentrated natural latex or concentrated natural skim latex.
7. The method according to claim 5, It is characterized in that The silane coupling agent is selected from one or more of γ-aminopropyl triethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane, γ-mercaptopropyl trimethoxysilane, bis-(γ-triethoxysilylpropyl)-tetrasulfide, bis-(γ-triethoxysilylpropyl)-disulfide, and γ-mercaptopropyl-ethoxybis(propyl-hexapropoxy)siloxane; The emulsifier is selected from one or more of sodium lauryl sulfate, dodecylphenol polyoxyethylene ether, nonylphenol polyoxyethylene ether, polyethylene glycol, stearic acid monoethanolamide, and fatty alcohol polyoxyethylene ether; The rubber lubricant is selected from one or more of talcum powder, mica powder, calcium carbonate, clay, and calcium terephthalate.
8. The method according to claim 5, It is characterized in that In the step (3), the second mixed liquid is placed on a high-temperature flash evaporation device for flocculation and rapid dehydration and drying, wherein the high-temperature flash evaporation device comprises a high-temperature flash evaporation roller, wherein the high-temperature flash evaporation roller has a cylindrical shell structure and an inner cavity, wherein the inner cavity stores heat transfer oil to ensure uniform heating of the surface of the high-temperature flash evaporation roller; The high-temperature flash evaporation device also includes a baffle groove, a mold temperature controller for providing heating, and a third motor for driving the high-temperature flash evaporation round roller to roll at a uniform speed. The rotation speed of the high-temperature flash evaporation round roller is 10-100r / min, and its surface temperature is 135-145°C.
9. The method according to claim 8, It is characterized in that When the second mixed liquid is transported to the surface of the high-temperature flash roller at a temperature of 135-145°C through the baffle groove, its water evaporates rapidly to form a molded rubber compound that adheres to the surface of the high-temperature flash roller and rolls with the high-temperature flash roller. When it rolls 5-8 times and the surface of the rubber compound is tight and has no obvious sticky lumps, the drying is completed, and the dried mother film is scraped off to complete the flocculation and dehydration cycle.
10. The method according to claim 5, It is characterized in that In the step (1), the rotation speed of the helical agitator and the main blade is 10000 r / min, and the rotation speed of the stirring tank is 100 r / min; in the step (2), the rotation speed of the helical agitator and the main blade is set to 20000 r / min, and the rotation speed of the stirring tank is 200 r / min.