Bonding method of silica gel product

The silicone products and the adhesives are processed through the plasma machine to form new chemical bonds to achieve glue-free bonding, which solves the problems of adhesive blockage and harmful substances, improves the yield and production efficiency of silicone products, is suitable for large-scale production and guarantees The product is environmentally friendly and safe.

CN118977423AInactive Publication Date: 2024-11-19GUANGDONG KANBAY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411106662.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When used to bond with adhesive during the production process, existing silicone products are prone to clogging fine pores or pipes, resulting in unqualified finished products. The adhesive has volatile irritating and harmful substances, affecting production efficiency and product safety.

Method used

The silicone products and the adhesive are processed by plasma machines, and new chemical bonds are formed by vacuum and hot press bonding to achieve glue-free bonding, ensuring firm bonding and high accuracy.

Benefits of technology

It improves the yield and production efficiency of silicone products, avoids the use of glue, reduces production costs and the content of harmful substances, is suitable for large-scale production, and ensures the environmental protection and safety of the products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991022020000051
    Figure BDA0004991022020000051
  • Figure BDA0004991022020000052
    Figure BDA0004991022020000052
  • Figure BDA0004991022020000061
    Figure BDA0004991022020000061
Patent Text Reader

Abstract

The invention provides a silica gel product bonding method which comprises the following steps: S1, putting a silica gel product and a bonded object into a plasma machine according to requirements, setting the vacuum degree to be-10 to-100kpa and the flow to be 100 to 350sccm, and treating for 8 to 30 seconds under certain power; and S2, taking out the silica gel product treated in the step S1 and the bonded object from the plasma machine, and carrying out hot-pressing lamination at a certain temperature until the silica gel product and the bonded object are firmly bonded, the bonded object contains atoms capable of forming bonds with Si atoms or O atoms in the silica gel product. The method is easy to operate and high in bonding precision, pores or pipelines of the silica gel products cannot be blocked, and the yield and production efficiency of the silica gel products are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicone product manufacturing, in particular to a method for bonding silicone products. Background Art

[0002] With the development of society, silicone products are increasingly appearing in people's field of vision due to their excellent performance, such as baby pacifiers, human trachea, etc.

[0003] There are some silicone products on the market, such as silicone airbags and products with hollow special-shaped channels, which must be formed separately and then bonded together during the production process. When adhesives are used to bond these silicone products, it is easy to block the pores or pipes of the silicone products, resulting in unqualified finished products that need to be reworked, which inevitably reduces the yield and production efficiency of silicone products. In addition, many adhesives are volatile and irritating, and may also contain harmful substances such as toluene; if the eyes are accidentally exposed to them, the hard glue after curing will also hurt the eyeballs. Therefore, it is particularly important to invent a method that can accurately bond silicone products firmly and ensure a good yield. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method that does not require the use of silicone glue and can accurately and firmly bond silicone products and ensure a good yield rate. The method is simple and feasible, easy to operate, has high bonding accuracy, and is suitable for large-scale production.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for bonding a silicone product comprises the following steps:

[0007] S1 puts the silicone product and the bonded object into the plasma machine as required, sets the vacuum degree to -10~-100kpa, the flow rate to 100~350sccm, and processes for 8~30S at a certain power;

[0008] S2: taking the silicone product and the adherend processed in step S1 out of the plasma machine, and performing hot pressing bonding at a certain temperature until the silicone product and the adherend are firmly bonded;

[0009] The adherend contains atoms that can form bonds with Si atoms or O atoms in the silica gel product, such as Si, Cu, Al, Fe, O atoms, etc.

[0010] In the present invention, when the silicone product and the adherend are three-dimensional structures or special shapes, the silicone product and the adherend need to be mounted on a specific fixture and then placed in the plasma machine. The processing time of the silicone product and the adherend in the plasma machine will be affected by the size and thickness of the silicone product and the adherend.

[0011] In the present invention, the adherend is one of silica gel, glass, metal and plastic.

[0012] In the present invention, the power in step S1 is adaptively changed according to the size of the plasma machine, and the power is 1 to 600W.

[0013] In the present invention, the temperature of the heat pressing bonding in the further step S2 is 50-200°C.

[0014] In the present invention, the pressure of the hot pressing bonding in step S2 is 10 to 170 KPa, and the time of the hot pressing bonding is 30 to 300 seconds.

[0015] In principle, the silicone product of the present invention and the adherend can be bonded at room temperature and pressure after being processed according to step S1. However, if the pressure is too small and the hot pressing bonding temperature is too low, the bonding will take a long time. For the sake of production efficiency, the best temperature for hot pressing bonding is generally 100-180°C, the best pressure is 120-170KPa, and the best time for hot pressing bonding is 50-120S. Too much pressure and too high temperature can easily cause the silicone product or the adherend to deform, affecting the quality of the product.

[0016] In the present invention, the metal is one of aluminum, copper and iron.

[0017] When the adherend is metal, the surface of the adherend must be kept clean before it is placed in the plasma machine in step S1. The surface of the metal workpiece cannot be touched by hands or other objects.

[0018] In the present invention, the plastic is one of PP, ABS, PBT, PPSU, PET, TPU, EVA, PES, PC, PA, and POM.

[0019] The reaction mechanism of the present invention is:

[0020] The present invention places the silicone product and the adherend into a plasma machine and processes them for a period of time under predetermined conditions, so that the polymer molecular bonds of the silicone in the silicone product are broken and the silicon-oxygen bonds are forged to form an ionic state. When the silicon-oxygen atoms in the ionic state encounter ions in the adherend that can be combined with them (such as silicon atoms and aluminum atoms), new chemical bonds are formed, which firmly locks the ions of the adherend and bonds the adherends.

[0021] The advantages and beneficial effects of the present invention are as follows:

[0022] 1. The bonding method of a silicone product of the present invention uses a plasma machine to process the silicone and the adherend so that the silicone and the adherend can be firmly bonded, is easy to operate, has high bonding accuracy, will not block the pores or pipes of the silicone product, and greatly improves the yield and production efficiency of the silicone product.

[0023] 2. The bonding method of the silicone product of the present invention is simple and feasible, avoids the use of silicone glue, reduces the production cost and the content of VOC in the silicone finished product, is more environmentally friendly and feasible, and is suitable for large-scale production. DETAILED DESCRIPTION

[0024] The present invention will be further described below with reference to specific embodiments, but is not limited thereto.

[0025] The present specific embodiment provides a method for bonding a silicone product, comprising the following steps:

[0026] S1 puts the silicone product and the adherend into the plasma machine as required, sets the vacuum degree to -10~-100KPa, the flow rate to 100~350sccm, and processes for 8~30S at a certain power; the power set is adjusted according to the size of the plasma machine, and the power can generally be set to 1~600W;

[0027] S2: taking the silicone product and the adherend processed in step S1 out of the plasma machine, and performing hot pressing bonding at a temperature of 50 to 200° C. until the silicone product and the adherend are firmly bonded;

[0028] The adherend contains atoms that can form bonds with Si atoms or O atoms in the silicone product.

[0029] In this specific embodiment, the adherend is one of silicone, glass, metal, and plastic.

[0030] When the silicone product and the adherend are three-dimensional structures or special shapes (such as silicone airbags, silicone pacifiers, etc.), the silicone product and the adherend must be installed on a specific fixture and then placed in the plasma machine.

[0031] 1. Tensile test

[0032] In a specific embodiment of the present invention, in order to facilitate the testing of the bonding strength between the silicone product and the adherend, a flat sample is selected for both the silicone product and the adherend, and the sample size is 50*15*1.2mm. During hot pressing and laminating, the silicone product and the adherend need to be partially laminated along the length direction, and the overlapping portion of the bonding is 20mm, and the exposed unbonded ends are convenient for tensile testing. In step S2 of this specific embodiment, hot pressing and laminating can also be carried out at room temperature and pressure, but in order to save the time of bonding the silicone product and the adherend, the temperature of hot pressing and laminating is generally selected to be 100-180°C, the pressure of hot pressing and laminating is 120-170KPa, and the time of hot pressing and laminating is 30-60S. After hot pressing and laminating, it needs to be placed for 1 hour for the finished product to cool before the tensile test.

[0033] This experiment conducted 20 groups of experiments for different silicone products and adherends, and the experimental conditions are shown in Table 1; in each group of embodiments, 5 silicone products and 5 adherends were selected for parallel testing and bonded into 5 finished products (respectively recorded as A, B, C, D, and E), and tensile tests were performed, and the test data were recorded in Table 2. The tensile test of this embodiment uses a machine produced by Dongguan Zhiqu Precision Instrument Co., Ltd., model ZQ-990LB.

[0034] Table 1 Bonding conditions of silicone products and adherends in Examples 1-20

[0035]

[0036] Table 2 Tensile test results of silicone products and adherends after bonding in Examples 1-20

[0037]

[0038]

[0039] According to Table 1 and Table 2, silicone products and adherends such as silicone, glass, metal, and plastic can be bonded together after being processed in a plasma machine, and all have a certain bonding strength, meeting the requirements of daily silicone bonding technology.

[0040] 2. Air tightness test

[0041] Install 8 groups of semi-finished silicone airbag tubes and the other half of the matching silicone airbag tubes on a specific fixture, and put them into the plasma machine as required, set the vacuum degree of the plasma machine to -25Kpa, the flow rate to 200sccm, and the processing time to 10s; take the processed silicone airbag tubes out of the plasma machine, and perform hot pressing and bonding at a temperature of 120°C and a pressure of 150kpa for 50s to form a silicone airbag tube finished product F.

[0042] After hot pressing, let it stand for one hour and then conduct an airtightness test after cooling.

[0043] In addition, eight groups of semi-finished silicone airbag tubes and the other half of the matching silicone airbag tubes are glued together to form airbag tube finished product G. After the glue is air-dried and firmly bonded, it is left to stand for one hour, and then an airtightness test is performed.

[0044] The results of the air tightness test showed that the 8 finished silicone airbag tubes F had no leakage, and the tracheal tubes were not blocked; the 8 finished silicone airbag tubes G had no leakage, but 3 of them had tracheal tubes blocked; it can be seen that the silicone products and the bonded objects treated in the plasma machine not only have good bonding effects, but also will not have tube or pore blockage when the products are special-shaped or three-dimensional structures (silicone tubes, pacifiers), which shows that the bonding method of the silicone products of the present invention can also greatly improve the product yield.

Claims

1. A method for bonding silicone products, Features The following steps are involved: S1 puts the silicone product and the bonded object into the plasma machine as required, sets the vacuum degree to -10~-100KPa, the flow rate to 100~350sccm, and processes for 8~30S at a certain power; S2: taking the silicone product and the adherend processed in step S1 out of the plasma machine, and performing hot pressing bonding at a certain temperature until the silicone product and the adherend are firmly bonded; The adherend contains atoms that can form bonds with Si atoms or O atoms in the silicone product.

2. The bonding method of silicone products according to claim 1, Features The adherend is one of silica gel, glass, metal and plastic.

3. The bonding method of silicone products according to claim 1, Features The power in step S1 is adaptively changed according to the size of the plasma machine, and the power is 1-600W.

4. The bonding method of silicone products according to claim 1, Features The temperature of the hot pressing bonding in step S2 is 50-200°C.

5. The bonding method of the silicone product according to claim 1 or 4, Features The pressure of the hot pressing bonding in step S2 is 10 to 170 KPa, and the time of the hot pressing bonding is 30 to 300 seconds.

6. The bonding method of silicone products according to claim 2, Features The metal is one of aluminum, copper and iron.

7. The bonding method of silicone products according to claim 2, Features When the adherend is metal, the surface of the adherend must be kept clean before being placed in the plasma machine in step S1.

8. The bonding method of silicone products according to claim 2, Features The plastic is one of PP, ABS, PBT, PPSU, PET, TPU, EVA, PES, PC, PA, and POM.

Citation Information

Patent Citations

  • Super-flexible base film served as graphene film carrier, and preparation method thereof

    CN106427145A

  • Fast bonding process of silica gel and PET

    CN109401646A

  • Metal and non-metal surface bonding method

    CN109664517A

  • Glass, metal, and rubber sheet gluing method, airplane glass, and preparation method thereof

    CN110205040A

  • Heat insulation pads with enhanced adhesion

    CN218857888U

Cited By

  • Bonding method for silicone product

    WO2026036578A1