Preparation method and application of large-aperture molecular sieve
By hydrothermal reaction and roasting of materials such as ethyl orthosilicate, ethanol, aluminum chloride hexahydrate and ethylenediamine, a large pore size Y-type molecular sieve was prepared, which solved the problem of insufficient adsorption of weak acid carbon dioxide by molecular sieve, and achieved the goal of achieving the Highly efficient water and carbon dioxide adsorption properties.
Patent Information
- Application Number
- CN202411179363.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
AI Technical Summary
The existing molecular sieve has a low adsorption of weakly acidic carbon dioxide, and its adsorption performance needs to be improved to meet industrial needs.
Materials such as ethyl orthosilicate, ethanol, aluminum chloride hexahydrate and ethylenediamine are mixed and dissolved, and large pore size Y-shaped molecular sieve is prepared through hydrothermal reaction and roasting process. The ammonia-p-silicon aluminum particles are decomposed and released. The internal structure is modified to improve the pore capacity and pore size, thereby improving adsorption performance.
The prepared molecular sieve has high pore volume, pore size and specific surface area, and shows good water adsorption and CO2 adsorption properties, meeting the needs of industrial applications.
Smart Images

Figure CN118978169A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous materials, and in particular to a preparation method of a large-pore molecular sieve and application thereof. Background Art
[0002] Molecular sieves have been widely used in industry as catalysts or catalyst carriers for different acid-catalyzed reactions such as catalytic cracking, hydrocracking, isomerization and alkylation. The properties and functions of molecular sieves mainly depend on their own silicon-aluminum skeleton ratio and the corresponding pore structure. The higher the silicon-aluminum ratio, the stronger the thermal stability and the greater the tolerance to acid. In addition, its hydrophilicity and hydrophobicity also change with the increase of the silicon-aluminum ratio, which in turn affects the adsorption performance of the molecular sieve. Molecular sieves with topological structures have moderate specific surface area and pore size, good stability, and simple preparation methods, making them a research hotspot in the field of carbon dioxide adsorption. However, the adsorption capacity of molecular sieve raw powder for weakly acidic carbon dioxide is low. Molecular sieves modified with organic bases show stronger affinity and adsorption capacity for water and carbon dioxide. In this work, molecular sieves were modified with organic bases to improve the adsorption performance of molecular sieves for water and carbon dioxide. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing a molecular sieve with a large pore size and its application. The preparation method provided by the present invention has a simple process and the obtained molecular sieve has a high pore volume, pore size and specific surface area.
[0004] In order to achieve the above object, the present invention adopts the following technical solution: The present invention provides a method for preparing a large-pore molecular sieve, comprising the following steps: (1) Mix a certain amount of ethyl orthosilicate solution and ethanol solution and stir them thoroughly; (2) Weighing an appropriate amount of aluminum chloride hexahydrate, adding it and stirring it thoroughly to completely hydrolyze it to obtain a precursor solution; (3) Add an indefinite amount of ethylenediamine solution into the precursor solution and stir evenly; (4) subjecting the obtained solution to ultrasonic treatment, and then placing it in a reactor for hydrothermal reaction; (5) After the reaction is completed, the solution is centrifuged, dried and ground; (6) The obtained powder is calcined to obtain the large-pore molecular sieve.
[0005] 1. A method for preparing a large pore molecular sieve, characterized in that it comprises the following steps: (1) Mix a certain amount of ethyl orthosilicate solution and ethanol solution and stir them thoroughly; (2) Weighing an appropriate amount of aluminum chloride hexahydrate, adding it and stirring it thoroughly to completely hydrolyze it to obtain a precursor solution; (3) Add an indefinite amount of ethylenediamine solution into the precursor solution and stir evenly; (4) subjecting the obtained solution to ultrasonic treatment, and then placing it in a reactor for hydrothermal reaction; (5) After the reaction is completed, the solution is centrifuged, dried and ground to obtain the Y-type molecular sieve with large pore volume and large pore size; (6) The obtained powder is calcined to obtain the large-pore molecular sieve.
[0006] Preferably, the solution in step (1) is tetraethyl orthosilicate and ethanol in a molar ratio of 9:171.
[0007] Preferably, the molar ratio of aluminum chloride to ethylenediamine in step (2) and step (3) is 0.7-0.8:0.2-2 Preferably, the temperature of the hydrothermal reaction in step (4) is 180°C and the reaction time is 12 h.
[0008] Preferably, the calcination process in step (6) may or may not be performed. If calcination is performed, the temperature is 500-550°C and the calcination time is 6 hours.
[0009] The invention provides a method for preparing a large-pore Y-type molecular sieve, wherein an aluminum source, a silicon source, ethanol and a modifier ethylenediamine are mixed and dissolved, and ethylenediamine is used to decompose and release ammonia to modify the internal structure of the formed silicon-aluminum particles, thereby obtaining silicon-aluminum particles with larger pore volume and pore size, thereby achieving controllable regulation of pore volume, pore size and specific surface area. The molecular sieve provided by the invention has good water adsorption and CO2 adsorption performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 is the X-ray diffraction pattern of the molecular sieve in Example 1; Figure 2 is a scanning electron microscope image of the molecular sieve in Example 1; Figure 3 is a thermogravimetric graph of carbon dioxide of the molecular sieve in Example 1; Figure 4 is the N2 adsorption isotherm of the molecular sieve in Example 1; Figure 5 is the N2 adsorption isotherm of the molecular sieve in Example 2; Figure 6 is the X-ray diffraction pattern of the molecular sieve in Example 3; Figure 7 is the N2 adsorption isotherm of the molecular sieve in Example 3; Figure 8 is the N2 adsorption isotherm of the molecular sieve in Example 4; Fig. 9 is the N2 adsorption isotherm of the molecular sieve in Example 5; Fig.10 This is a thermogravimetric graph of carbon dioxide of the molecular sieve in Example 5; Fig.11 is the X-ray diffraction pattern of the molecular sieve in Example 6; Fig.12 is a scanning electron microscope image of the molecular sieve in Example 6; Fig.13 This is the N2 adsorption isotherm of the molecular sieve in Example 6. DETAILED DESCRIPTION
[0011] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0012] The molar ratio of the used ethyl orthosilicate, ethanol solution, aluminum chloride hexahydrate and ethylenediamine is 9:171:3.5-4:1-10.
[0013] Example 1 Take 1.8 ml of tetraethyl orthosilicate (SiO2 content is 28%) and 34.2 ml of ethanol solution (C2H5OH mass fraction is 95%) respectively, stir thoroughly and add 0.7141 g of aluminum chloride (AlCl3•6H2O, mass fraction is 98%), stir until the aluminum chloride is completely hydrolyzed, then perform ultrasound for 1 hour, and immediately transfer to a hydrothermal kettle for hydrothermal reaction. The temperature of the hydrothermal reaction is 180 ° C and the reaction time is 12 h. After the reaction is completed, the solution is centrifuged and washed (repeatedly washed with deionized water 3 times), dried (60 ° C overnight), and ground into powder to obtain the molecular sieve. The molecular sieve prepared in this example was subjected to X-ray diffraction, and the results are as follows Figure 1 As shown in FIG. 1 , the diffraction peak is a silicon oxide phase structure. The molecular sieve prepared in this embodiment is subjected to electron scanning, and the electron microscope image obtained is as follows: Figure 2 As shown, irregular pores of about 5 nm can be seen on its surface. Figure 3 The carbon dioxide thermogravimetric curve of the molecular sieve in Example 1 shows good carbon dioxide adsorption performance. Its pore volume is 0.75 cm3 / g, pore diameter is 5.8 nm, specific surface area is 474.89 m2 / g, and water adsorption is 28.19%.
[0014] Example 2 Take 1.8 ml of tetraethyl orthosilicate (SiO2 content is 28%) and 34.2 ml of ethanol solution (C2H5OH mass fraction is 95%), stir thoroughly and add 0.7141 g of aluminum chloride (AlCl3•6H2O, mass fraction is 98%), stir until aluminum chloride is completely hydrolyzed, then ultrasonicate for 1 hour, and immediately transfer to a hydrothermal kettle for hydrothermal reaction. The temperature of the hydrothermal reaction is 180 ℃ and the reaction time is 12 h. After the reaction, the solution is centrifuged (washed repeatedly with deionized water 3 times), dried (60 ℃ overnight), ground into powder, and then the powder is placed in a muffle furnace for roasting (550 ℃, 6 h) to obtain the molecular sieve. Its pore volume is 0.80 cm3 / g, the pore diameter is 7.7 nm, and the specific surface area is 375.58 m2 / g. Example 3 Take 1.8 ml of tetraethyl orthosilicate (SiO2 content is 28%) and 34.2 ml of ethanol solution (C2H5OH mass fraction is 95%) respectively, stir thoroughly and add 0.7141g of aluminum chloride (AlCl3•6H2O, mass fraction is 98%), stir until the aluminum chloride is completely hydrolyzed, then add 0.5 ml of ethylenediamine (mass fraction is 98%) and stir vigorously for a long time, then ultrasonicate for 1 hour, and immediately transfer to a hydrothermal kettle for hydrothermal reaction. The temperature of the hydrothermal reaction is 180 ° C and the reaction time is 12 h. After the reaction is completed, the solution is centrifuged and washed (deionized water is repeatedly washed 3 times), dried (60 ° C overnight), and ground into powder to obtain the molecular sieve. Its pore volume is 1.06 cm3 / g, the pore diameter is 20.20nm, and the specific surface area is 203.05 m2 / g. The molecular sieve prepared in this example was subjected to X-ray diffraction, and the results are as follows Figure 6 As shown, the diffraction peak is the silicon oxide phase structure.
[0015] Example 4 Take 1.8 ml of tetraethyl orthosilicate (SiO2 content is 28%) and 34.2 ml of ethanol solution (C2H5OH mass fraction is 95%), stir thoroughly, add 0.7141g of aluminum chloride (AlCl3•6H2O, mass fraction is 98%), stir until aluminum chloride is completely hydrolyzed, then add 0.5 ml of ethylenediamine (mass fraction is 98%), stir vigorously for a long time, and then ultrasonicate for 1 hour, and immediately transfer to a hydrothermal kettle for hydrothermal reaction. The temperature of the hydrothermal reaction is 180 ℃ and the reaction time is 12 h. After the reaction is completed, the solution is centrifuged and washed (deionized water is repeatedly washed 3 times), dried (60 ℃ overnight), and ground into powder. Then the powder is placed in a muffle furnace for roasting (550 ℃, 6h) to obtain the Y-type molecular sieve. Its pore volume is 0.72 cm3 / g, the pore diameter is 6.18nm, and the specific surface area is 414.06 m2 / g. Example 5 Take 1.8 ml of ethyl orthosilicate (SiO2 content is 28%) and 34.2 ml of ethanol solution (C2H5OH mass fraction is 95%), stir thoroughly, add 0.7141g of aluminum chloride (AlCl3•6H2O, mass fraction is 98%), stir until aluminum chloride is completely hydrolyzed, then add 2 ml of ethylenediamine (mass fraction is 98%), stir vigorously for a long time, and then perform ultrasonic treatment for 1 hour, and immediately transfer to a hydrothermal kettle for hydrothermal reaction, the temperature of the hydrothermal reaction is 180 ℃, and the reaction time is 12 h. After the reaction is completed, the solution is centrifuged and washed (deionized water is repeatedly washed 3 times), dried (60 ℃ overnight), and ground into powder to obtain the molecular sieve. Fig.10 The carbon dioxide thermogravimetric curve of the molecular sieve in Example 5 shows good carbon dioxide adsorption performance. Its pore volume is 1.06 cm3 / g, pore diameter is 20.65 nm, and specific surface area is 198.03m2 / g. Example 6 Take 1.8 ml of tetraethyl orthosilicate (SiO2 content is 28%) and 34.2 ml of ethanol solution (C2H5OH mass fraction is 95%), stir thoroughly, add 0.7141 g of aluminum chloride (AlCl3•6H2O, mass fraction is 98%), stir until aluminum chloride is completely hydrolyzed, then add 0.5 ml of ethylenediamine (mass fraction is 98%), stir vigorously for a long time, and then perform ultrasonic treatment for 1 hour, and immediately transfer to a hydrothermal kettle for hydrothermal reaction, the temperature of the hydrothermal reaction is 180 ℃, and the reaction time is 12 h. After the reaction is completed, the solution is centrifuged and washed (deionized water is repeatedly washed 3 times), dried (60 ℃ overnight), and ground into powder, and then the powder is placed in a muffle furnace for roasting (550 ℃, 6h), and the Y-type molecular sieve is obtained. The pore volume is 1.03 cm3 / g, the pore diameter is 20.75 nm, and the specific surface area is 191.76 m2 / g. The molecular sieve prepared in this example was subjected to X-ray diffraction, and the results are as follows: Fig.11 As shown in FIG. 1 , the diffraction peak is a silicon oxide phase structure. The molecular sieve prepared in this embodiment is subjected to electron scanning, and the electron microscope image obtained is as follows: Fig.12 As shown, irregular pores of about 20 nm can be seen on its surface.
[0016] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0017] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a large pore molecular sieve, characterized in that: The method comprises the following steps: (1) mixing a certain amount of tetraethyl orthosilicate solution and ethanol solution and stirring them thoroughly; (2) weighing an appropriate amount of aluminum chloride hexahydrate, adding the mixture and stirring the mixture thoroughly to completely hydrolyze the mixture, thereby obtaining a precursor solution; (3) adding a certain amount of ethylenediamine solution to the precursor solution and stirring the mixture uniformly; (4) subjecting the obtained solution to ultrasonic treatment and then placing the mixture in a reactor for hydrothermal reaction; (5) centrifuging, drying and grinding the solution after the reaction is completed; and (6) calcining the obtained powder to obtain the large-pore molecular sieve.
2. The preparation method according to claim 1, characterized in that The solution described in step (1) is ethyl orthosilicate and ethanol, and the molar ratio thereof is 9:
171.
3. The preparation method according to claim 1, characterized in that: The molar ratio of aluminum chloride to ethylenediamine in step (2) and step (3) is 0.7-0.8:0.2-2.
4. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction in step (4) is 180°C and the reaction time is 12 h.
5. The preparation method according to claim 1, characterized in that The roasting process described in step (6) may or may not be performed. If roasting is performed, the temperature is 500-550°C and the roasting time is 6 hours.