Preparation method and application of novel negative thermal expansion material
By preparing Yb2W3O12:Nd3+ film material, the energy transfer of Nd3+→Yb3+ is achieved using 808nm excitation light, the existing negative thermal expansion materials are solved, and the problem of unstable at room temperature and low excitation absorption rate of 980nm is achieved with high efficiency and low cost new negative Thermal expansion material, suitable for temperature sensors and integrated circuits in the medical and communications fields.
Patent Information
- Application Number
- CN202411065467.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing negative thermal expansion materials are metastable at room temperature, are easy to decompose, and have a low absorption rate of 980nm light excitation, which limits their application in the medical and communication fields, especially in near-infrared spectroscopy.
By preparing Yb2W3O12:Nd3+ film material, using an 808nm excitation light source, the energy transfer of Nd3+→Yb3+ is achieved, and it is significantly luminous, and sintered in the opal template to form a stable new negative thermal expansion material.
It improves the absorption rate under 808nm excitation, has stable material performance and low cost, is suitable for large-scale production, and realizes controllable regulation of Nd3+ ion luminescence, and is suitable for temperature sensors and integrated circuit applications in the medical and communication fields.
Smart Images

Figure CN118978181A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic non-metallic materials, and in particular to a preparation method and application of a novel negative thermal expansion material. Background Art
[0002] Most materials in nature have the property of thermal expansion and contraction, but there is also the abnormal phenomenon of "thermal contraction and cold expansion" in nature, that is, negative thermal expansion. Different expansion coefficients between materials will cause device fatigue, performance degradation or even permanent failure. With the development of science and technology, people have an increasing demand for materials with low or zero expansion coefficients. People hope to achieve the purpose of compounding positive and negative expansion materials into zero or low expansion materials by studying negative thermal expansion (NTE) materials. Negative thermal expansion materials in nature are still very limited, and there are very few negative thermal expansion materials with excellent performance and engineering application value. At present, regarding negative thermal expansion materials, for unknown materials, the urgent problem we face is to actively find new negative thermal expansion materials and explore effective preparation methods; for existing negative thermal expansion materials, the urgent problem we face is to implement effective performance regulation, such as appropriately lowering the temperature phase transition point, achieving zero expansion and controllable expansion coefficients, etc. For example, the oxide negative thermal expansion materials that are widely studied include ZrW2O8, a common AM2O8 material. However, ZrW2O8 is a metastable phase material at room temperature, undergoes a phase transition at around 150°C, and is prone to decomposition when compounded with other materials, which seriously restricts its application. Lanthanide ion-doped upconversion luminescence experiments (nanocrystals, films, etc.) have the characteristics of efficient near-infrared (NIR) upconversion, low luminescence background interference, and negligible biological toxicity. They have been widely used in biological fields such as bioimaging, biosensing, and drug delivery. However, water, an important component of organisms, has strong absorption in the near-infrared spectrum around 970nm, which limits the optical application of 980nm response. Therefore, 808nm light excitation is used to minimize the risk of overheating.
[0003] Therefore, it is very necessary and of great significance to develop a new thin film material with stable 808nm excited negative expansion performance, simple process and suitable for large-scale production. Summary of the invention
[0004] The purpose of the present invention is to design a method for preparing a new negative thermal expansion material that can convert low-energy excitation light into high-energy luminescence, produce obvious negative thermal expansion phenomenon through excitation by 808nm excitation light source, and has good sensitivity and reversibility.
[0005] In order to achieve the above object, the present invention is implemented by the following technical scheme: A method for preparing a new type of negative thermal expansion material, characterized in that it comprises the following steps:
[0006] A method for preparing a novel negative thermal expansion material, characterized in that it comprises the following steps:
[0007] S1. preparing an opal template: using a quartz sheet as a substrate, treating the substrate, placing the treated substrate in a polystyrene sol liquid, and heating it at a constant temperature for 3 to 5 days, thereby obtaining an opal template;
[0008] S2. Prepare a precursor solution: weigh Yb2O3 and Nd2O3 in a molar ratio of Yb2O3:Nd2O3=287-574:18.3-36.6, put the weighed Yb2O3 and Nd2O3 into a beaker, then add 20-30 mL of concentrated nitric acid into the beaker, heat and dissolve to obtain a nitrate solution; heat the obtained nitrate solution to evaporate the water in the nitrate solution to obtain a gel-like mixture of Yb(NO3)3 and Nd(NO3)3; after the mixture is fully cooled, add 2-4 mL of anhydrous ethanol, stir well and let stand to obtain a clear Yb2W3O 12 :Nd 3+ Precursor solution;
[0009] S3. Use a pipette to draw 20-30 μl of Yb2W3O 12 :Nd 3+ The precursor sol is dropped onto the surface of the template and allowed to evenly penetrate into the opal template. The precursor sol is sintered in an air atmosphere at 800 to 900° C. for 2.5 to 3.5 hours to obtain a new type of negative thermal expansion material.
[0010] Further, in S1, the substrate for preparing the opal template is a quartz sheet, comprising the following steps:
[0011] S1.1. Preparation of polystyrene sol liquid: clean several 25 mm × 25 mm weighing bottles, add 7 ml of deionized water to each clean weighing bottle, then drop 500 μl of 654 band gap monodisperse polystyrene microsphere suspension into each weighing bottle, finally place the solution in each weighing bottle in an ultrasonic disperser for ultrasonic dispersion, and take out after ultrasonic dispersion for 1 to 2 hours to obtain polystyrene sol liquid;
[0012] S1.2, substrate cleaning: take out several quartz pieces and soak them in a mixed solution of concentrated sulfuric acid and hydrogen peroxide for 1 to 2 hours to perform surface cleaning and surface activity treatment, then rinse the residual acid on the surface with clean water until the pH is neutral, and finally wash and soak with deionized water to obtain a substrate;
[0013] S1.3, take out the substrates soaked in S1.2 one by one, and vertically insert them into the polystyrene sol liquid along the wall of the volumetric flask, with 2 to 4 substrates inserted symmetrically into each flask;
[0014] S1.4. Place the volumetric flask containing the quartz plate obtained in S1.3 into an electric thermostatic box at 50-60°C for 3-5 days to obtain the opal template.
[0015] Another object of the present invention is to provide an application of a new type of negative thermal expansion material, characterized in that the new type of negative thermal expansion material is applied in the fields of medical treatment and communication.
[0016] Furthermore, the new negative thermal expansion material is applied in the medical and communication fields, specifically in temperature sensors and integrated circuits;
[0017] The application principle is: the new negative thermal expansion material can achieve Nd 3+ →Yb 3+ The energy transfer enables the new negative thermal expansion material to emit significant light in the near-infrared range.
[0018] The beneficial effects of the present invention are:
[0019] The present invention prepares a new type of negative thermal expansion material film. Compared with the negative thermal expansion material excited by 980nm, the negative thermal expansion material excited by 808nm has higher absorption rate, wider application and lower cost. At the same time, the synthesis method of the new negative thermal expansion material has good repeatability and reliability. It can change the Nd 3+ The luminescence of ions is regulated; the invention has low cost, is expected to be applied in the fields of medical treatment, communication, etc., and is expected to realize industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0021] Figure 1 This is an XRD picture of the new negative thermal expansion material prepared in Example 1 of the present invention;
[0022] Figure 2 This is a picture of the structure of the opal template prepared in Embodiment 1 of the present invention;
[0023] Figure 3 This is a structural picture of the new negative thermal expansion material prepared in Embodiment 1 of the present invention;
[0024] Figure 4 This is a spectrum picture of the new negative thermal expansion material prepared in embodiment 1 of the present invention under 808nm laser irradiation.
[0025] Figure 5 This is a temperature-varying spectrum picture of the new negative thermal expansion material prepared in Example 1 of the present invention under 808nm laser irradiation.
[0026] Figure 6 This is a temperature sensitivity diagram of the new negative thermal expansion material prepared in Example 1 of the present invention at 20-300°C under 808nm laser irradiation and temperature. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] This embodiment describes a specific preparation method of a new type of negative thermal expansion material, and the steps are as follows:
[0030] S1. Preparation of opal template:
[0031] S1.1. Preparation of polystyrene sol liquid: clean several 25 mm × 25 mm weighing bottles, add 7 ml of deionized water to each clean weighing bottle, then drop 500 μl of 654 band gap monodisperse polystyrene microsphere suspension into each weighing bottle, finally place the solution in each weighing bottle in an ultrasonic disperser for ultrasonic dispersion, and take out after ultrasonic dispersion for 1 to 2 hours to obtain polystyrene sol liquid;
[0032] S1.2, substrate cleaning: take out several quartz plates and soak them in a mixed solution of concentrated sulfuric acid and hydrogen peroxide for 2 hours to perform surface cleaning and surface activity treatment, then rinse the residual acid on the surface with clean water until the pH is neutral, and finally wash and soak with deionized water to obtain a substrate;
[0033] S1.3, take out the substrates soaked in S1.2 one by one, and vertically insert them into the polystyrene sol liquid along the wall of the volumetric flask, with 3 substrates inserted symmetrically into each flask;
[0034] S1.4. Place the volumetric flask containing the quartz plate obtained in S1.3 into an electric thermostatic box at 55°C for 3 to 5 days to obtain the opal template.
[0035] S2. Preparation of precursor solution:
[0036] Weighed Yb2O3 (m = 2.8g) and Nd2O3 (m = 0.2g) were placed in a beaker (the molar ratio of Yb2O3 to Nd2O3 was 287:18.3), and then 20mL of concentrated nitric acid was added to the beaker and heated to dissolve to obtain a nitrate solution; the obtained nitrate solution was heated to evaporate the water in the nitrate solution to obtain a gel-like mixture of Yb(NO3)3 and Nd(NO3)3; after the mixture was fully cooled, 2ml of anhydrous ethanol was added, and after fully stirring, it was allowed to stand to obtain a clear Yb2W3O 12 :Nd 3+ Precursor solution;
[0037] S3, use a pipette to draw 30 μl of Yb2W3O 12 :Nd 3+ The precursor sol is dropped on the surface of the template, and evenly infiltrated into the opal template. The new negative thermal expansion material is obtained by sintering it in an air atmosphere at 850°C for 3 hours.
[0038] Example 2
[0039] This example describes the specific application of the new negative thermal expansion material prepared in Example 1, as follows:
[0040] The new negative thermal expansion material was placed at the 808 nm semiconductor laser irradiation position, and the new negative thermal expansion material was irradiated by an 808 nm semiconductor laser (steady-state / transient fluorescence spectrometer (Edinburgh FLS1000)); Figure 3 The results show that the new negative thermal expansion material prepared by the present invention can achieve Nd under 808nm laser irradiation. 3+ →Yb 3+ The energy transfer of the new negative thermal expansion material enables it to emit light significantly in the near-infrared range; the thermal enhancement of the new negative thermal expansion material is attributed to Yb2W3O 12 The lattice shrinks, which results in the 3+ To Yb 3+ The energy transfer of ions is increased and phonons are assisted, with good reversibility. Under 808nm excitation, Nd 3+ The typical emission spectrum of ions can be controlled.
[0041] The specific application principle of temperature measurement in the fields of medical treatment and communication is as follows:
[0042] Prepared negative thermal expansion material film Yb2W3O 12 :Nd 3+ Application as temperature measurement:
[0043] The negative thermal expansion material phosphor Yb2W3O 12 :Nd3+ The sample was heated at 20℃, 60℃, 100℃, 140℃, 180℃, 220℃, 260℃ and 300℃, and the fluorescence spectrum was obtained by using FLS980 steady-state / transient fluorescence spectrometer. From the spectrum, it can be seen that the near-infrared (975nm, 1058nm, 1330nm) gradually increases with the increase of temperature, indicating that the fluorescence intensity is dependent on temperature. Therefore, we can measure the temperature through the relationship between fluorescence intensity and temperature.
[0044] The absolute temperature sensitivity Sr is used to indicate the rate of change of the FIR value with temperature:
[0045]
[0046] The sensitivity increases first and then decreases with the increase of temperature, such as Figure 6 It shows a temperature dependence with a maximum absolute sensitivity of 0.6% K at 573 K. -1 , proving the feasibility of temperature measurement.
Claims
1. A method for preparing a novel negative thermal expansion material, characterized in that: The steps include: S1. preparing an opal template: using a quartz sheet as a substrate, treating the substrate, placing the treated substrate in a polystyrene sol liquid, and heating it at a constant temperature for 3 to 5 days, thereby obtaining an opal template; S2. Prepare a precursor solution: weigh Yb2O3 and Nd2O3 in a molar ratio of Yb2O3:Nd2O3=287-574:18.3-36.6, put the weighed Yb2O3 and Nd2O3 into a beaker, then add 20-30 mL of concentrated nitric acid into the beaker, heat and dissolve to obtain a nitrate solution; heat the obtained nitrate solution to evaporate the water in the nitrate solution to obtain a gel-like mixture of Yb(NO3)3 and Nd(NO3)3; after the mixture is fully cooled, add 2-4 mL of anhydrous ethanol, stir well and let stand to obtain a clear Yb2W3O 12 :Nd 3+ Precursor solution; S3. Use a pipette to draw 20-30 μl of Yb2W3O 12 :Nd 3+ The precursor sol is dropped onto the surface of the template and allowed to evenly penetrate into the opal template. The precursor sol is sintered in an air atmosphere at 800 to 900° C. for 2.5 to 3.5 hours to obtain a new type of negative thermal expansion material.
2. The method for preparing a novel negative thermal expansion material according to claim 1, characterized in that: In S1, the substrate for preparing the opal template is a quartz sheet, comprising the following steps: S1.
1. Preparation of polystyrene sol liquid: clean several 25 mm × 25 mm weighing bottles, add 7 ml of deionized water to each clean weighing bottle, then drop 500 μl of 654 band gap monodisperse polystyrene microsphere suspension into each weighing bottle, finally place the solution in each weighing bottle in an ultrasonic disperser for ultrasonic dispersion, and take out after ultrasonic dispersion for 1 to 2 hours to obtain polystyrene sol liquid; S1.2, substrate cleaning: take out several quartz pieces and soak them in a mixed solution of concentrated sulfuric acid and hydrogen peroxide for 1 to 2 hours to perform surface cleaning and surface activity treatment, then rinse the residual acid on the surface with clean water until the pH is neutral, and finally wash and soak with deionized water to obtain a substrate; S1.3, take out the substrates soaked in S1.2 one by one, and vertically insert them into the polystyrene sol liquid along the wall of the volumetric flask, with 2 to 4 substrates inserted symmetrically into each flask; S1.
4. Place the volumetric flask containing the quartz plate obtained in S1.3 into an electric thermostatic box at 50-60°C for 3-5 days to obtain the opal template.
3. Application of a new type of negative thermal expansion material, characterized in that: The new negative thermal expansion material is used in the fields of medicine and communications.
4. The use of a new type of negative thermal expansion material according to claim 3, characterized in that: Application of the novel negative thermal expansion material in the medical and communication fields, specifically in temperature sensors and integrated circuits; The application principle is: the new negative thermal expansion material can achieve Nd 3+ →Yb 3+ The energy transfer enables the new negative thermal expansion material to emit significant light in the near-infrared range.
Citation Information
Patent Citations
Preparation method of negative-thermal-expansion material Y2W3O12 thin film
CN105331935A
Erbium-ytterbium co-doped phosphotungstic acid scandium zirconium two-dimensional negative thermal expansion material with moisture resistance and anomalous enhanced luminescence and preparation method thereof
CN115093223A
Rare earth doped negative thermal expansion luminescent material and preparation method and application thereof
CN116004231A
Cited By
SiO2 coated negative thermal expansion film and application thereof
CN119735380A
A SiO2-coated negative thermal expansion film and its application
CN119735380B