Large-diameter ferrite circular ring and production process thereof

By employing a two-stage ball milling and slurry injection molding process, the manufacturing challenges of large-diameter ferrite rings in existing technologies have been solved, enabling efficient and low-cost production of ferrite rings and improving their magnetic properties.

CN118978394AInactive Publication Date: 2024-11-19ANHUI ONE MAGNET ELECTRONIC CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411066407.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies make it difficult to manufacture large-diameter ferrite rings with an outer diameter exceeding 300 mm, and the production process is complex and costly.

Method used

The process employs a two-stage ball milling and slurry injection molding process, including steps such as raw material mixing, ball milling, pre-firing, precipitation, hydraulic molding, and high-temperature sintering, which controls material consumption and mold size and simplifies the process flow.

Benefits of technology

This technology enables the efficient production of large-diameter ferrite rings, reduces costs, improves magnetic properties, and simplifies the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978394A_ABST
    Figure CN118978394A_ABST
Patent Text Reader

Abstract

The invention discloses a large-diameter ferrite circular ring and a production process thereof, and belongs to the technical field of rare earth magnetic materials. Comprising the following steps: mixing preparation raw materials and water, performing primary ball-milling processing, performing pre-sintering through a pre-sintering furnace, performing crushing and sieving to obtain pre-sintered material particles, mixing silicon dioxide, calcium carbonate and the pre-sintered material particles, performing secondary ball-milling processing, performing precipitation in a precipitation tank, and performing injection molding on water-containing precipitation slurry to obtain a finished product. According to the method, two times of ball milling processing and a slip casting method are adopted, high-precision size control can be achieved, meanwhile, the surface quality is controlled, few waste materials are generated in the production process, the technological process is simple, and the large-diameter ferrite circular ring can be conveniently prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth magnetic materials, and in particular to a large-diameter ferrite ring and a production process thereof. Background Art

[0002] Ferrite ring, also known as ferrite magnetic ring, is an important device used in electronic and communication equipment to suppress electromagnetic interference (EMI) or radio frequency interference (RFI). Large diameter ferrite ring is a magnetic material that is widely used in various equipment, such as large audio, household appliances, automotive motors, and medical equipment. Ferrite is a ceramic material mainly composed of iron oxide (Fe2O3) and other metal elements. It has the characteristics of high resistivity and high magnetic permeability, and can effectively absorb and dissipate high-frequency electromagnetic waves. Ferrite materials are widely used in electromagnetic compatibility (EMC) due to their ability to adjust magnetic and electrical properties.

[0003] At present, the process of manufacturing permanent magnet ferrite rings in China can only produce ferrite rings with a maximum outer diameter of 300mm. Secondly, the existing process is complicated and the cost of production line investment is high, and the practicality is poor. Therefore, a new process for preparing large-diameter ferrite rings is needed, which can increase the diameter of ferrite rings while reducing production costs. Summary of the invention

[0004] The purpose of the present invention is to provide a large-diameter ferrite ring and a production process thereof, so as to solve the problems in the background technology that the process is complicated, the investment cost is high and the ferrite ring with an outer diameter exceeding 300 mm cannot be manufactured.

[0005] A large-diameter ferrite ring and a production process thereof, characterized in that the steps include:

[0006] Step 1, fully mixing the prepared raw materials and water, and then performing a ball milling process to obtain a ball milling slurry;

[0007] Step 2, pre-sintering the primary ball-milled slurry in a pre-sintering furnace and crushing and sieving to obtain pre-sintered material particles;

[0008] Step 3, the silicon dioxide, calcium carbonate and pre-calcined material particles are fully mixed and then subjected to secondary ball milling to obtain a secondary ball milling slurry;

[0009] Step 4, placing the secondary ball-milled slurry in a precipitation tank for precipitation to obtain an aqueous precipitation slurry;

[0010] Step 5, injecting the water-containing precipitation slurry into a grouting molding mold through a hydraulic molding machine for compression molding to obtain a large-diameter ferrite ring blank;

[0011] Step 6, drying the large diameter ferrite ring blank and sintering it at high temperature to obtain a large diameter ferrite ring sintered blank;

[0012] Step 7: Grind and spray the large diameter ferrite ring to obtain a large diameter ferrite ring.

[0013] Furthermore, in step 1, the raw materials are ferric oxide and rare earth oxides.

[0014] Furthermore, in step 1, the volume ratios of the ball milling medium, water, ferric oxide and rare earth oxide are 60-70%: 20-30%: 3-5%: 3-5%.

[0015] Furthermore, in step 1, the ball milling medium is bearing steel with a diameter of 6 mm and a hardness of HRC>55, the ball mill speed is 18-22 r / min, and the ball milling time is 9-11 h.

[0016] Furthermore, in step 2, the pre-burning temperature is 900-1000° C., the pre-burning time is 2 hours, and the mesh size of the crushed and sieved sieve is 100 meshes.

[0017] Furthermore, in step 3, the volume proportions of the ball milling medium, water, pre-sintered material particles, calcium carbonate and silicon dioxide are 50-60%: 20-30%: 10-20%: 5-10%: 5-10%.

[0018] Furthermore, in step 4, the secondary ball milling slurry precipitation time is 3-4 days, and the water content of the obtained aqueous precipitation slurry is 32-40%.

[0019] Furthermore, in step 5, the hydraulic forming machine is a 300-ton four-column hydraulic forming machine, the one-time forming time is 5-8 minutes, the forming magnetic field is ≥50,000 ampere-turns, and the outer diameter of the obtained large-diameter permanent magnet ferrite ring blank is Φ400 mm.

[0020] Furthermore, in step 6, the drying treatment is carried out at room temperature with ventilation drying for 25-30 days until the moisture content of the large-diameter ferrite ring blank is ≤5%, the sintering temperature is 1200-1500° C., and the sintering time is 3 hours.

[0021] Furthermore, in step 7, the spraying process is to spray the large-diameter ferrite sintered blank all over.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention adopts two ball milling processes, which can improve the uniformity and fineness of the ball milling slurry particles, provide a good foundation for the subsequent sintering process, and the obtained large-diameter ferrite ring has the best magnetic properties.

[0024] 2. The present invention adopts slurry injection molding, which can accurately control material consumption and model size, reduce costs, simplify the process flow, and further improve the comprehensive magnetic properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a flow chart of a large-diameter ferrite ring and its production process according to an embodiment of the present application. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] See also Figure 1 , a large diameter ferrite ring and a production process thereof, comprising the following steps:

[0029] Step 1, fully mixing ferric oxide, rare earth oxide and water and then performing a ball milling process to obtain a ball milling slurry, wherein the volume ratio of ball milling medium, water, ferric oxide and rare earth oxide is 60%:30%:5%:5%, the ball mill speed is 18r / min, and the ball milling time is 9h;

[0030] Step 2, pre-calcining the once-milled slurry at 950° C. for 2 h in a pre-calcining furnace, and crushing and sieving to obtain pre-calcined material particles;

[0031] Step 3, the silicon dioxide, calcium carbonate and pre-burned material particles are fully mixed and then subjected to secondary ball milling to obtain a secondary ball milling slurry, wherein the volume ratios of the ball milling medium, water, pre-burned material particles, calcium carbonate and silicon dioxide are 50%:30%; 10%:5%:5%, the ball mill speed is 20r / min, and the ball milling time is 9h;

[0032] Step 4, placing the secondary ball-milled slurry in a precipitation tank for precipitation to obtain a water-containing precipitation slurry with a water content of 32%;

[0033] Step 5, injecting the aqueous precipitation slurry into a grouting molding mold through a hydraulic molding machine for compression molding to obtain a large-diameter ferrite ring blank;

[0034] Step 6, drying the large diameter ferrite ring blank and sintering it at 1200° C. to obtain a large diameter ferrite ring sintered blank;

[0035] Step 7: Grind and spray the large diameter ferrite ring to obtain a large diameter ferrite ring.

[0036] Example 2

[0037] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that in step 1, the volume ratios of ball milling medium, water, ferric oxide and rare earth oxide are 70%:20%:5%:5%, the ball mill speed is 18 r / min, the ball milling time is 9 h, and the other components and parameters remain unchanged.

[0038] Example 3

[0039] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that in step 3, the volume proportions of ball milling medium, water, pre-sintered material particles, calcium carbonate and silicon dioxide are 55%: 25%: 10%: 5%: 5%, the ball mill speed is 20 r / min, the ball milling time is 9 hours, and the other components and parameters remain unchanged.

[0040] Example 4

[0041] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that in step 3, the volume proportions of ball milling medium, water, pre-sintered material particles, calcium carbonate and silicon dioxide are 60%: 20%: 10%: 5%: 5%, the ball mill speed is 20 r / min, the ball milling time is 9 h, and the other components and parameters remain unchanged.

[0042] Example 5

[0043] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that in step 3, the volume ratios of ball milling medium, water, pre-sintered material particles, calcium carbonate and silicon dioxide are 50%: 20%: 10%: 10%: 10%, the ball mill speed is 20 r / min, the ball milling time is 9 h, and the other components and parameters remain unchanged.

[0044] Example 6

[0045] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that in step 3, the volume ratios of ball milling medium, water, pre-sintered material particles, calcium carbonate and silicon dioxide are 50%: 20%: 20%: 5%: 5%, the ball mill speed is 22 r / min, the ball milling time is 11 h, and the other components and parameters remain unchanged.

[0046] Example 7

[0047] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that in step 4, the secondary ball-milled slurry is placed in a precipitation tank for precipitation to obtain a water-containing precipitation slurry with a water content of 36%, and the other components and parameters remain unchanged.

[0048] Example 8

[0049] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that in step 4, the secondary ball-milled slurry is placed in a precipitation tank for precipitation to obtain a water-containing precipitation slurry with a water content of 40%, and the other components and parameters remain unchanged.

[0050] Example 9

[0051] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that the temperature of high-temperature sintering in step 6 is 1500° C., and the other components and parameters remain unchanged.

[0052] Comparative Example 1

[0053] A large-diameter ferrite ring and a production process thereof, wherein the process flow is the same as that of Example 1, except that steps 4-5 are omitted, and the large-diameter ferrite ring blank is obtained by using an oscillating die to mold the secondary ball-milled slurry, while other components and parameters remain unchanged.

[0054] The magnet properties of the above different embodiments and comparative examples were tested at 25° C. The test results are shown in Table 1.

[0055] Table 1

[0056]

[0057] It can be seen from Table 1 that the higher the volume proportion of the ball milling medium in the primary ball milling and the secondary ball milling, the better the comprehensive magnetic properties of the large-diameter ferrite rings obtained. A high proportion of ball milling medium can improve the ball milling efficiency and reduce energy consumption, while ensuring the uniformity and fineness of the magnet components, providing a good foundation for the subsequent sintering process. The obtained slurry has the best magnetic properties and the slurry particle size distribution is good. At the same time, increasing a certain sintering temperature can effectively improve the comprehensive magnetic properties. It can be seen from Comparative Example 1 that the comprehensive magnetic properties of the large-diameter ferrite obtained by vibration pressing molding are significantly lower than those of the large-diameter ferrite obtained by slurry injection molding.

[0058] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0059] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A large diameter ferrite ring and its production process, characterized in that: The following steps are involved: Step 1, fully mixing the prepared raw materials and water, and then performing a ball milling process to obtain a ball milling slurry; Step 2, pre-sintering the primary ball-milled slurry in a pre-sintering furnace and crushing and sieving to obtain pre-sintered material particles; Step 3, the silicon dioxide, calcium carbonate, water and pre-burned material particles are fully mixed and then ball-milled for a second time to obtain a secondary ball-milled slurry; Step 4, placing the secondary ball-milled slurry in a precipitation tank for precipitation to obtain an aqueous precipitation slurry; Step 5, injecting the aqueous precipitation slurry into a grouting molding mold through a hydraulic molding machine for compression molding to obtain a large-diameter ferrite ring blank; Step 6, drying the large diameter ferrite ring blank and sintering it at high temperature to obtain a large diameter ferrite ring sintered blank; Step 7: Grind and spray the large diameter ferrite ring to obtain a large diameter ferrite ring.

2. A large diameter ferrite ring and its production process according to claim 1, characterized in that: In the step 1, the raw materials are ferric oxide and rare earth oxide; in the step 1, the volume proportions of ball milling medium, water, ferric oxide and rare earth oxide are 60-70%: 20-30%: 3-5%: 3-5%.

3. A large diameter ferrite ring and its production process according to claim 3, characterized in that: The ball milling medium is bearing steel with a diameter of 6 mm and a hardness of HRC>55. The ball mill speed is 18-22 r / min and the ball milling time is 9-11 h.

4. A large diameter ferrite ring and its production process according to claim 1, characterized in that: In the step 2, the pre-burning temperature is 900-1000° C., the pre-burning time is 2 hours, and the mesh size of the crushed and sieved sieve is 100 meshes.

5. A large diameter ferrite ring and its production process according to claim 1, characterized in that: In step 3, the volume proportions of ball milling medium, water, pre-sintered material particles, calcium carbonate and silicon dioxide are 58-60%: 18-20%: 12-14%: 2-4%: 2-4%.

6. A large diameter ferrite ring and its production process according to claim 1, characterized in that: In step 4, the secondary ball milling slurry precipitation time is 3-4 days, and the water content of the obtained aqueous precipitation slurry is 32-40%.

7. A large diameter ferrite ring and its production process according to claim 1, characterized in that: In step 5, the hydraulic forming machine is a 300-ton four-column hydraulic forming machine, the one-time forming time is 5-8 minutes, the forming magnetic field is ≥50,000 ampere-turns, and the outer diameter of the obtained large-diameter permanent magnet ferrite ring blank is Φ400 mm.

8. A large diameter ferrite ring and its production process according to claim 1, characterized in that: In step 6, the drying treatment is carried out at room temperature with ventilation drying for 25-30 days until the moisture content of the large-diameter ferrite ring blank is ≤5%, the sintering temperature is 1200-1500° C., and the sintering time is 3 hours.

9. A large diameter ferrite ring and its production process according to claim 1, characterized in that: In the step 7, the spraying treatment is to spray the large-diameter ferrite sintered blank all over.

10. A large diameter ferrite ring, characterized in that: Prepared by the process described in any one of claims 1 to 10.

Citation Information

Patent Citations

  • Ferrite preparation method and prepared ferrite thereby

    CN104496452A

  • Production technology and production assembly line for permanent magnetic ferrite ring with large diameter

    CN105523752A

  • Preparation method of permanent ferrite material

    CN110372365A